Diamond wire and preparation method thereof

By loading a hydrophilic sealant on the surface of the diamond wire, the problems of poor liquid carrying capacity and difficult chip removal after thinning of the diamond wire are solved, the cutting efficiency and product quality are improved, and the use cost is reduced.

CN118927428APending Publication Date: 2024-11-12CHANGSHA DIAT NEW MATERIAL SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411084881.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

After the diamond wire is thinned, the liquid-carrying capacity is weakened, making it difficult to discharge the silicon chips produced during the cutting of the silicon wafer, resulting in poor cutting efficiency and product quality.

Method used

The surface of the diamond wire is loaded with a hydrophilic sealant, and the fatty alcohol polyoxyethylene ether M, isoocrystalline polyoxypropylene ether, carbon 9-11 primary alcohol 8 ethoxylate and 1,9 -Nanodene glycol and other materials form a closed layer to improve the liquid-carrying capacity and chip removal performance of the diamond wire.

Benefits of technology

It improves the cutting ability of diamond wire, reduces silicon chip adhesion, significantly improves cutting efficiency and product quality, and reduces usage costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118927428A_ABST
    Figure CN118927428A_ABST
Patent Text Reader

Abstract

The invention relates to a hydrophilic sealing agent diamond wire and a preparation method thereof, and belongs to the technical field of diamond wires, a bus is cleaned, the treated bus is pre-electroplated to form a plating layer, diamond sand particles are combined with the plating layer of the bus, and then combination of diamond and the plating layer is stabilized. And finally, the electroplated bus forms a hydrophilic layer on the steel wire body through a soaking or coating method. And covering the wire body with the hydrophilic layer, and drying to obtain the hydrophilic diamond wire. In the diamond wire production process, a hydrophilic sealing agent is used for covering a diamond wire plating layer, the contact angle between the diamond wire and the sealing agent can be reduced, the flowing capacity of liquid on the diamond wire is improved, monocrystalline silicon chippings on the diamond wire can be taken away, and the cutting capacity of the diamond wire is enhanced. The process can be compatible with an existing diamond wire preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of wire cutting wires, and in particular relates to a diamond wire and a preparation method thereof. Background Art

[0002] Diamond wire cutting is an advanced cutting technology that mainly uses diamond wire as a cutting tool. It is used in the cutting of high-hardness and brittle materials, such as photovoltaic silicon wafers and sapphire.

[0003] When cutting silicon wafers, the diamond wire is installed on the cutting machine and rotated at high speed. The diamond particles fixed on the steel wire will do the cutting work. The diamond wire is pressed on the surface of the material to be cut, and the diamond particles move at high speed driven by the steel wire, producing a grinding effect, thereby cutting off part of the material. Compared with the traditional mortar cutting method, diamond wire cutting has higher efficiency and better cutting quality. Because the diamond wire has diamond micro-teeth, this increases the cutting ability of the steel wire, making the cutting speed faster and the cutting surface smoother.

[0004] At present, the overall trend of diamond wire is thinning. The advantages of thinning are as follows: 1. The waste generated during cutting is reduced, thereby reducing silicon costs.

[0005] 2. Reduce the stress generated during cutting and improve the product yield.

[0006] However, there are also certain problems with thinning the wire, such as the weakening of the diamond wire's ability to carry liquid, and the difficulty in removing silicon chips generated when cutting silicon wafers. Therefore, a method of efficiently improving the diamond wire's ability to carry liquid, remove silicon chips, and cutter force is currently being sought to solve the above technical problems. Summary of the invention

[0007] A first object of the present invention is to provide a diamond wire having high liquid carrying capacity, silicon chip removal capacity and cutting force.

[0008] The second object of the present invention is to provide a method for preparing the diamond wire.

[0009] The third object of the present invention is to provide an application of the diamond wire.

[0010] The present invention is achieved through the following technical solutions: A diamond wire, the surface of which is loaded with a sealing agent; the sealing agent is obtained by drying a sealing solution; the sealing solution comprises 15-25wt% of fatty alcohol polyoxyethylene ether M and 1-5wt% of 2-ethylhexanol EoPo copolymer.

[0011] The sealing solution also includes 15-25 wt % of isooctyl alcohol polyoxyethylene polyoxypropylene ether 9.

[0012] The sealing solution also includes 5-10 wt% of carbon 9-11 primary alcohol 8 ethoxylate.

[0013] The blocking solution further includes 1-5 wt % of 1,9-nonanediol.

[0014] The blocking solution further includes 1-5 wt % of 1,9-nonanediol.

[0015] The sealing solution further comprises 15-25 wt % of isooctyl alcohol polyoxyethylene polyoxypropylene ether 9, 5-10 wt % of carbon 9-11 primary alcohol 8 ethoxylate and 1-5 wt % of 1,9-nonanediol.

[0016] The method for preparing the diamond wire comprises the following steps: Pre-plating the surface of the diamond wire to form a pre-plating layer; Through electroplating, the pre-plated layer formed by pre-electroplating on the surface of the diamond wire is combined with the diamond sand; Further electroplating is performed to form a plating layer on the surface of the pre-plating layer; The plated diamond wire is immersed in a sealing solution and then dried to form a sealing layer on the surface of the coating.

[0017] The temperature of the sealing solution is 50°C to 60°C.

[0018] Using the water bath heating method, first add deionized water and heat it to 50℃~60℃, then add the above materials.

[0019] The blocking solution is heated in a water bath.

[0020] The diamond wire is applied to wire cutting.

[0021] Compared with the prior art, the present invention has the following beneficial effects: The hydrophilic sealant loaded on the surface of the diamond wire provided by the present invention increases the contact angle between the diamond wire and the sealant, reduces the adhesion of silicon chips and cuttings on the diamond wire, and improves the cutting ability of the diamond wire. At the same time, the sealant can also improve the liquid carrying ability of the diamond wire. It can be seen that the diamond wire provided by the present invention solves the problem of enhancing the cutting ability of the diamond wire on the basis of thinning the diamond wire.

[0022] The present invention adds a non-surfactant in the continuous production process of the diamond wire, so that a water layer similar to the non-surfactant is formed on the surface of the diamond wire when passing through the sealant tank, thereby producing a hydrophilic sealant diamond wire. The present invention provides a good diamond wire cutting effect and can significantly reduce the use cost thereof. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A flow chart of the preparation of diamond wire is shown.

[0024] Figure 2 A longitudinal schematic diagram of the diamond wire provided in Example 1 is shown.

[0025] Figure 3 A lateral schematic diagram of the diamond wire provided in Example 1 is shown. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] In order to solve the problem of poor liquid carrying capacity and difficulty in chip removal after diamond wire is thinned, the present invention provides a diamond wire, the surface of the diamond wire is loaded with a sealing agent; the sealing agent is obtained by drying a sealing solution; the sealing solution comprises 15-25wt% of fatty alcohol polyoxyethylene ether M and 1-5wt% of 2-ethylhexanol EoPo copolymer. The sealing solution also comprises 15-25wt% of isooctyl alcohol polyoxyethylene polyoxypropylene ether 9. The sealing solution also comprises 5-10wt% of carbon 9-11 primary alcohol 8 ethoxylate. The sealing solution also comprises 1-5wt% of 1,9-nonanediol. The sealing solution also comprises 1-5wt% of 1,9-nonanediol. The sealing solution also comprises 15-25wt% of isooctyl alcohol polyoxyethylene polyoxypropylene ether 9, 5-10wt% of carbon 9-11 primary alcohol 8 ethoxylate and 1-5wt% of 1,9-nonanediol.

[0028] The surface of the diamond wire provided by the present invention is loaded with a closed layer, and the materials selected for the closed layer are all substances with polar groups and strong hydrophilicity to water. Fatty alcohol polyoxyethylene ether M has good decontamination and lubrication effects as a non-ionic surfactant. Isooctyl alcohol polyoxyethylene polyoxypropylene ether 9 is a non-ionic surfactant with low surface tension (surface tension is proportional to surface energy) and good solubility. Carbon 9-11 primary alcohol 8 ethoxylate is a non-ionic surfactant, which does not dissociate when dissolved in water. The lipophilic group in its molecule is basically the same as that of the ionic surfactant, and it also contains a certain amount of oxygen-containing hydrophilic groups such as hydroxyl groups. Since the non-ionic surfactant does not exist in an ionic state, it has high stability, is not easily affected by the presence of strong electrolytes, is not easily affected by acids and alkalis, and has good compatibility with other surfactants, does not strongly adsorb on the solid surface, and has good washing, dispersion, foaming, and wetting. There are hydroxyl groups at both ends of 1,9-nonanediol, which has good hydrophilicity. 2-Ethylhexanol EoPo copolymer is used as a dispersant.

[0029] The invention also provides a hydrophilic sealing agent diamond wire and a preparation method thereof.

[0030] like Figure 1 As shown, the method may include the following steps: A1, clean the diamond wire. The cleaning process includes alkali cleaning, water cleaning, acid cleaning, and No. 2 water cleaning. The main purpose is to remove the oily substances, oxide layer and dust on the diamond wire.

[0031] The diamond wires used are high carbon steel and tungsten wires with a wire diameter of 28 μm to 35 μm.

[0032] A2, pre-plating the surface of the diamond wire to form a pre-plating layer on the surface.

[0033] A3, after the second coating is applied on the pre-coating, the corundum and the coating are bonded. The sand mold used for the corundum is 5 sand / 5.5 sand / 6 sand / 6.5 sand A4, the third electroplating is carried out to form a coating to stabilize the consolidation of the diamond grains and the coating.

[0034] A5, diamond wire is electroplated with a sealant by forming a water layer on the surface of the diamond wire through an infiltration method or a coating method. This sealant is used to reduce the contact angle between the diamond wire and the sealant.

[0035] The contact angle refers to the angle between the solid-liquid interface, the liquid interior and the gas-liquid interface at the interface of solid, liquid and gas, as shown in the figure. The larger the contact angle, the more hydrophobic it is, and the smaller the contact angle, the more hydrophilic it is.

[0036] Cutting fluid refers to the liquid medium used when diamond wire is used to cut silicon wafers, etc. The functions of cutting fluid include cooling and chip removal. The inventors have found that when the contact angle between the diamond wire and the cutting fluid decreases, it becomes more hydrophilic, and the diamond wire can bring more cutting fluid into the saw seam when cutting silicon wafers, that is, improve the liquid carrying capacity. Since the cutting fluid contains detergents and wetting agents, if there is more cutting fluid in the saw seam, it can take away more silicon grains generated when cutting silicon wafers, commonly known as cutting debris, thereby improving the chip removal capacity.

[0037] In an optional embodiment, the raw materials used to prepare the sealing agent include: one or more of fatty alcohol polyoxyethylene ether M, isooctyl alcohol polyoxyethylene polyoxypropylene ether 9, carbon 9-11 primary alcohol 8 ethoxylate, 1,9-nonanediol, and 2-ethylhexanol EoPo copolymer.

[0038] A6, heat the diamond wire in an oven at 150-200℃.

[0039] The present invention is further described below in conjunction with specific embodiments.

[0040] The CAS number of the 2-ethylhexanol EoPo copolymer involved in the embodiment of the present invention is 64366-70-7 The CAS of fatty alcohol polyoxyethylene ether M is 37335-03-8 The CAS number of 2-isooctanol polyoxyethylene polyoxypropylene ether 9 is 64366-70-7 Example 1 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0041] The wire diameter of the diamond wire is 38μm, the sand mold is 6 sand, and it undergoes pre-plating, sanding and thickening in sequence, with respective currents of 4.7A, 19.2A and 38.8A.

[0042] The electroplated diamond wire was placed in a sealing solution tank, into which 18% by mass of fatty alcohol polyoxyethylene ether M and 5% by mass of 2-ethylhexanol EoPo copolymer were added. Deionized water was first added and heated to 55° C. using a water bath heating method, and the above materials were then added.

[0043] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0044] Example 2 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0045] The wire diameter of the diamond wire is 38μm, the sand mold is 6 sand, and it undergoes pre-plating, sanding and thickening in sequence, with respective currents of 4.7A, 19.2A and 38.8A.

[0046] The electroplated diamond wire was placed in a sealing solution tank, into which 15% by mass of fatty alcohol polyoxyethylene ether M and 1% by mass of 2-ethylhexanol EoPo copolymer were added. Deionized water was first added and heated to 55° C. using a water bath heating method, and the above materials were added.

[0047] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0048] Example 3 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0049] The wire diameter of the diamond wire is 38μm, the sand mold is 6 sand, and it undergoes pre-plating, sanding and thickening in sequence, with respective currents of 4.7A, 19.2A and 38.8A.

[0050] The electroplated diamond wire was placed in a sealing solution tank, into which 25% by mass of fatty alcohol polyoxyethylene ether M and 5% by mass of 2-ethylhexanol EoPo copolymer were added. Deionized water was first added and heated to 55° C. using a water bath heating method, and the above materials were added.

[0051] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0052] Example 4 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0053] The wire diameter of the diamond wire is 38μm, the sand mold is 6 sand, and it undergoes pre-plating, sanding and thickening in sequence, with respective currents of 4.7A, 19.2A and 38.8A.

[0054] The electroplated diamond wire was placed in a sealing solution tank, to which 15% by mass of isooctyl alcohol polyoxyethylene polyoxypropylene ether 9, 15% by mass of fatty alcohol polyoxyethylene ether M and 1% by mass of 2-ethylhexanol EoPo copolymer were added. Deionized water was first added and heated to 55° C. using a water bath heating method, and the above materials were then added.

[0055] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0056] Example 5 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0057] The wire diameter of the diamond wire is 38μm, the sand mold is 6 sand, and it undergoes pre-plating, sanding and thickening in sequence, with respective currents of 4.7A, 19.2A and 38.8A.

[0058] The electroplated diamond wire was placed in a sealing solution tank, to which 25% by mass of isooctyl alcohol polyoxyethylene polyoxypropylene ether 9, 15% by mass of fatty alcohol polyoxyethylene ether M and 1% by mass of 2-ethylhexanol EoPo copolymer were added. Deionized water was first added and heated to 55° C. using a water bath heating method, and the above materials were then added.

[0059] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0060] Example 6 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0061] The wire diameter of the diamond wire is 38μm, the sand mold is 6 sand, and it undergoes pre-plating, sanding and thickening in sequence, with respective currents of 4.7A, 19.2A and 38.8A.

[0062] The electroplated diamond wire was placed in a sealing solution tank, to which 5% by mass of carbon 9-11 primary alcohol 8 ethoxylate, 18% by mass of fatty alcohol polyoxyethylene ether M and 5% by mass of 2-ethylhexanol EoPo copolymer were added. Deionized water was first added and heated to 55° C. using a water bath heating method, and the above materials were then added.

[0063] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0064] Example 7 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0065] The wire diameter of the diamond wire is 38μm, the sand mold is 6 sand, and it undergoes pre-plating, sanding and thickening in sequence, with respective currents of 4.7A, 19.2A and 38.8A.

[0066] The electroplated diamond wire was placed in a sealing solution tank, to which 10% by mass of carbon 9-11 primary alcohol 8 ethoxylate, 18% by mass of fatty alcohol polyoxyethylene ether M and 5% by mass of 2-ethylhexanol EoPo copolymer were added. Deionized water was first added and heated to 55° C. using a water bath heating method, and the above materials were then added.

[0067] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0068] Example 8 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0069] The wire diameter of the diamond wire is 38μm, the sand mold is 6 sand, and it undergoes pre-plating, sanding and thickening in sequence, with respective currents of 4.7A, 19.2A and 38.8A.

[0070] The electroplated diamond wire was placed in a sealing solution tank, to which 1% by mass of 1,9-nonanediol, 10% by mass of carbon 9-11 primary alcohol 8 ethoxylate, 18% by mass of fatty alcohol polyoxyethylene ether M and 5% by mass of 2-ethylhexanol EoPo copolymer were added. Deionized water was first added and heated to 55°C using a water bath heating method, and the above materials were then added.

[0071] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0072] Example 9 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0073] The wire diameter of the diamond wire is 38μm, the sand mold is 6 sand, and it undergoes pre-plating, sanding and thickening in sequence, with respective currents of 4.7A, 19.2A and 38.8A.

[0074] The electroplated diamond wire was placed in a sealing solution tank, to which were added 5% by mass of 1,9-nonanediol, 10% by mass of carbon 9-11 primary alcohol 8 ethoxylate, 18% by mass of fatty alcohol polyoxyethylene ether M and 5% by mass of 2-ethylhexanol EoPo copolymer. Deionized water was first added and heated to 55°C using a water bath heating method, and the above materials were then added.

[0075] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0076] Example 10 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0077] The wire diameter of the diamond wire is 38μm, the sand mold is 6 sand, and it undergoes pre-plating, sanding and thickening in sequence, with respective currents of 4.7A, 19.2A and 38.8A.

[0078] The electroplated diamond wire was placed in a sealing solution tank, to which 1% by mass of 1,9-nonanediol, 25% by mass of fatty alcohol polyoxyethylene ether M and 5% by mass of 2-ethylhexanol EoPo copolymer were added. Using a water bath heating method, deionized water was first added and heated to 55°C, and then the above materials were added.

[0079] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0080] Embodiment 11 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0081] The wire diameter of the diamond wire is 38μm, the sand mold is 6 sand, and it undergoes pre-plating, sanding and thickening in sequence, with respective currents of 4.7A, 19.2A and 38.8A.

[0082] The electroplated diamond wire was placed in a sealing solution tank, to which 5% by mass of 1,9-nonanediol, 25% by mass of fatty alcohol polyoxyethylene ether M and 5% by mass of 2-ethylhexanol EoPo copolymer were added. Using a water bath heating method, deionized water was first added and heated to 55°C, and then the above materials were added.

[0083] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0084] Example 12 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0085] The wire diameter of the diamond wire is 38μm, the sand mold is 6 sand, and it undergoes pre-plating, sanding and thickening in sequence, with respective currents of 4.7A, 19.2A and 38.8A.

[0086] The electroplated diamond wire was placed in a sealing solution tank, to which 5% by mass of 1,9-nonanediol, 25% by mass of fatty alcohol polyoxyethylene ether M and 5% by mass of 2-ethylhexanol EoPo copolymer were added. Using a water bath heating method, deionized water was first added and heated to 55°C, and then the above materials were added.

[0087] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0088] Example 13 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0089] The wire diameter of the diamond wire is 38μm, the sand mold is 6 sand, and it undergoes pre-plating, sanding and thickening in sequence, with respective currents of 4.7A, 19.2A and 38.8A.

[0090] The electroplated diamond wire was placed in a sealing solution tank, to which 5% by mass of 1,9-nonanediol, 25% by mass of fatty alcohol polyoxyethylene ether M and 5% by mass of 2-ethylhexanol EoPo copolymer were added. Using a water bath heating method, deionized water was first added and heated to 55°C, and then the above materials were added.

[0091] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0092] Embodiment 14 The diamond wire substrate is cleaned to remove surface oil and oxide layer, and the specific process includes alkali washing, water washing, acid washing and water washing.

[0093] The wire diameter of the diamond wire is 38μm, the sand type is 6 sand, and it is pre-plated, sanded and thickened in sequence, with respective currents of 4.7A, 19.2A and 38.8A The electroplated diamond wire was placed in a sealing solution tank, to which 18% by mass of fatty alcohol polyoxyethylene ether M, 2% by mass of 1,9-nonanediol, 20% by mass of isooctyl alcohol polyoxyethylene polyoxypropylene ether 9 and 5% by mass of 2-ethylhexanol EoPo copolymer were added. Deionized water was first added and heated to 50°C-60°C using a water bath heating method, and the above materials were added.

[0094] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0095] Embodiment 15 The diamond wire substrate is cleaned to remove oil and oxide layer on the surface. The specific process includes alkaline washing, water washing, acid washing and No. 2 water washing.

[0096] The wire diameter of the diamond wire is 38μm, the sand type is 6 sand, and it is pre-plated, sanded and thickened in sequence, with respective currents of 4.7A, 19.2A and 38.8A The electroplated diamond wire was placed in a sealing solution tank, to which 18% by mass of fatty alcohol polyoxyethylene ether M, 2% by mass of 1,9-nonanediol, 8% by mass of carbon 9-11 primary alcohol 8 ethoxylate and 5% by mass of 2-ethylhexanol EoPo copolymer were added. Deionized water was first added and heated to 50°C-60°C using a water bath heating method, and the above materials were added.

[0097] Finally, the water is dried in an oven at 150°C to obtain the finished product.

[0098] At the same time, in the process of preparing diamond wire, the temperature of water bath heating will also affect the contact angle of diamond wire.

[0099] Specifically, the ratio of the blocking solution is as follows: The weight percentage of the fatty alcohol polyoxyethylene ether M is 15% to 25% and the weight percentage of the 2-ethylhexanol EoPo copolymer is 1% to 5%.

[0100] Alternatively, the weight percentage of fatty alcohol polyoxyethylene ether M is 15% to 25%, the weight percentage of isooctyl alcohol polyoxyethylene polyoxypropylene ether 9 is 15% to 25%, and the weight percentage of 2-ethylhexanol EoPo copolymer is 1% to 5%.

[0101] The contact angle data of the diamond wire finally prepared by the water bath heating method are as follows.

[0102] The sequence number 6 is the best ratio for this method.

[0103] Specifically, the ratio of the blocking solution is as follows: The weight percentage of the fatty alcohol polyoxyethylene ether M is 15% to 25% and the weight percentage of the 2-ethylhexanol EoPo copolymer is 1% to 5%.

[0104] Alternatively, the weight percentage of fatty alcohol polyoxyethylene ether M is 15% to 25%, the weight percentage of carbon 9-11 primary alcohol 8 ethoxylate is 5% to 10%, and the weight percentage of 2-ethylhexanol EoPo copolymer is 1% to 5%.

[0105] The contact angle data of the diamond wire finally prepared by the water bath heating method are as follows.

[0106] The sequence number 6 is the best ratio for this method.

[0107] Specifically, the ratio of the blocking solution is as follows: 15% to 25% by mass of fatty alcohol polyoxyethylene ether M, 1% to 5% by mass of 1,9-nonanediol, 5% to 10% by mass of carbon 9-11 primary alcohol 8 ethoxylate and 1% to 5% by mass of 2-ethylhexanol EoPo copolymer.

[0108] The contact angle data of the diamond wire finally prepared by the water bath heating method are as follows.

[0109] The sequence number 3 is the best ratio for this method.

[0110] Specifically, the ratio of the blocking solution is as follows: The weight percentage of the fatty alcohol polyoxyethylene ether M is 15% to 25%, the weight percentage of 1,9-nonanediol is 1% to 5%, the weight percentage of isooctyl alcohol polyoxyethylene polyoxypropylene ether 9 is 15% to 25% and the weight percentage of 2-ethylhexanol EoPo copolymer is 1% to 5%.

[0111] The contact angle data of the diamond wire finally prepared by the water bath heating method are as follows.

[0112] The sequence number 2 is the best ratio for this method.

[0113] Specifically, the ratio of the blocking solution is as follows: 15% to 25% by mass of fatty alcohol polyoxyethylene ether M, 1% to 5% by mass of 1,9-nonanediol, 5% to 10% by mass of carbon 9-11 primary alcohol 8 ethoxylate, 15% to 25% by mass of isooctyl alcohol polyoxyethylene polyoxypropylene ether 9 and 1% to 5% by mass of 2-ethylhexanol EoPo copolymer.

[0114] The contact angle data of the diamond wire finally prepared by the water bath heating method are as follows.

[0115] The sequence number 2 is the best ratio for this method.

Claims

1. A diamond wire, Features: The surface of the diamond wire is loaded with a sealing agent; The blocking agent is obtained by drying the blocking solution; The sealing solution includes 15-25 wt % of fatty alcohol polyoxyethylene ether M and 1-5 wt % of 2-ethylhexanol EoPo copolymer.

2. The diamond wire according to claim 1, Features: The sealing solution also includes 15-25 wt % of isooctyl alcohol polyoxyethylene polyoxypropylene ether 9.

3. The diamond wire according to claim 1, Features: The sealing solution also includes 5-10 wt% of carbon 9-11 primary alcohol 8 ethoxylate.

4. The diamond wire according to claim 2, Features: The blocking solution further includes 1-5 wt % of 1,9-nonanediol.

5. The diamond wire according to claim 3, Features: The blocking solution further includes 1-5 wt % of 1,9-nonanediol.

6. The diamond wire according to claim 1, Features: The sealing solution further comprises 15-25 wt % of isooctyl alcohol polyoxyethylene polyoxypropylene ether 9, 5-10 wt % of carbon 9-11 primary alcohol 8 ethoxylate and 1-5 wt % of 1,9-nonanediol.

7. The method for preparing a diamond wire according to claim 1, Features: The steps include: Pre-plating the surface of the diamond wire to form a pre-plating layer; Through electroplating, the pre-plated layer formed by pre-electroplating on the surface of the diamond wire is combined with the diamond sand; Further electroplating is performed to form a plating layer on the surface of the pre-plating layer; The plated diamond wire is immersed in a sealing solution and then dried to form a sealing layer on the surface of the coating.

8. The method for preparing a diamond wire according to claim 7, Features: The temperature of the sealing solution is 50°C to 60°C. Using the water bath heating method, first add deionized water and heat it to 50℃~60℃, then add the above materials.

9. The method for preparing a diamond wire according to claim 7, Features: The blocking solution is heated in a water bath.

10. Use of the diamond wire according to claim 1, Features: Applicable to wire cutting.

Citation Information

Cited By

  • Diamond wire surface modification liquid, diamond wire surface modification method and diamond wire saw

    CN120250103A