Thermal-insulation fireproof composite material for building and preparation method of thermal-insulation fireproof composite material
Through the combination of modified flame retardant and fiber-based gel, the problem of insufficient fire resistance and environmental protection of traditional insulation materials is solved, and an efficient and environmentally friendly insulation and fire-proof composite material for building is achieved, with good flame retardant and thermal insulation effects.
Patent Information
- Application Number
- CN202410978347.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing thermal insulation materials for building use have shortcomings in fire resistance and environmental protection. Traditional organic materials will produce harmful substances, affecting the environment and human health, and the hygroscopicity and dust problems of inorganic materials will also affect their application.
The flame retardant was prepared by using 1,3,5-triformylphthalglucosol and p-phenylenediamine and 9,10-dihydro-9-oxa-10-phosphazepamphene-10-oxide. It is foamed with polyurethane, combined with hydrophobic treated silk fibroin fibers and modified carboxylated expanded graphite to form a fiber-based gel, and a fire-resistant layer-gel layer-fire-resistant layer structure is formed by freeze-drying.
It realizes the high mechanical properties and low thermal conductivity of the material, improves the flame retardant effect and thermal insulation performance, and reduces the harm to the environment and the human body, providing an efficient and environmentally friendly thermal insulation and fire-proof composite material for building.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal insulation material preparation, in particular to a thermal insulation and fireproof composite material for construction and a preparation method thereof. Background Art
[0002] With the acceleration of urbanization and the rapid development of the construction industry, the number of high-rise buildings and large public places is increasing. These places have a high density of people and are difficult to evacuate. Once a fire occurs, the consequences are disastrous. Therefore, it is very important to improve the fire resistance of buildings. Thermal insulation and fireproof composite materials can effectively inhibit the spread of fire, reduce the harm of fire to people and property, and protect people's lives and property.
[0003] Commonly used thermal insulation materials such as polyurethane and phenolic foam have the advantages of good thermal insulation performance, light weight, convenient construction, and good crack resistance, which can effectively prevent the generation of cracks. However, these materials have poor fire resistance, are easy to burn, and have high production costs. Some inorganic thermal insulation materials such as rock wool and glass wool have the advantages of good fire resistance, non-flammability, no harmful gases at high temperatures, and low cost. However, the disadvantage of inorganic thermal insulation materials is that they have high hygroscopicity and are easily affected by moisture, which affects their thermal insulation effect, and their fiber materials are prone to dust, which is harmful to the human body. In addition, some organic-inorganic composite materials also have good thermal insulation effects, such as polystyrene molded board (EPS) and extruded board (XPS), which have the advantages of good thermal insulation performance, relatively low price, and convenient construction. However, these materials will produce toxic gases during the combustion process, which will cause harm to the environment and human health.
[0004] As people's awareness of environmental protection continues to increase, the requirements for building materials are also getting higher and higher. Traditional insulation materials often use organic materials such as polystyrene and polyurethane. These materials will produce harmful substances during production and use, causing harm to the environment and human health. Insulation and fireproof composite materials use environmentally friendly materials such as inorganic materials or low-smoke halogen-free flame retardant materials, which can reduce pollution to the environment and harm to the human body.
[0005] Modern buildings have higher and higher requirements for thermal insulation performance. Thermal insulation materials can effectively reduce the heat loss of buildings, improve the energy efficiency of buildings, and reduce energy waste. At the same time, thermal insulation materials can also reduce the energy consumption of air-conditioning systems and reduce operating costs. Therefore, the research on thermal insulation and fireproof composite materials can provide an efficient and environmentally friendly thermal insulation solution for the construction industry. Summary of the invention
[0006] The object of the present invention is to provide a thermal insulation and fireproof composite material for construction and a preparation method thereof, so as to solve the problems raised in the background technology. 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is modified by using 1,3,5-triformylphloroglucinol and p-phenylenediamine, mixed with polyurethane for foaming to prepare a fireproof layer, and then the silk fibroin fiber is hydrophobically treated, and then mixed with dopamine-modified carboxylated expanded graphite to prepare a fiber-based gel. The gel is used to bond the fireproof layer and freeze-dried. The obtained thermal insulation and fireproof material has the characteristics of good mechanical properties and low thermal conductivity.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A method for preparing a thermal insulation and fireproof composite material for construction, comprising the following steps:
[0009] S1. Modifying 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide using 1,3,5-triformylphloroglucinol and p-phenylenediamine to obtain a modified flame retardant;
[0010] S2. Adding a modified flame retardant to the polyurethane material to prepare a fireproof layer;
[0011] S3, hydrophobic treatment of silk fibroin fibers, followed by mixing with dopamine-modified carboxylated expanded graphite to prepare a fiber-based gel;
[0012] S4. Coat the fiber-based gel on the surface of the fireproof layer, then spray a layer of oxidizing solution, and then use the fireproof layer to sandwich the fiber-based gel in the middle, apply pressure, fix, and then freeze-dry the material to form a fireproof layer-gel layer-fireproof layer structure, thereby obtaining a thermal insulation and fireproof composite material for construction.
[0013] Further, in step S1, the modified flame retardant is prepared by the following steps:
[0014] The trimethylbenzene and dioxane were mixed in a volume ratio of 1:1, and 1,3,5-triformylphloroglucinol and p-phenylenediamine were added after stirring evenly. After continuing to stir until evenly, 0.5 mL of 3 mol / L acetic acid solution was added, and the system temperature was increased to 50-90°C. After reacting for 8 hours, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, and the reaction was continued for 24 hours. Subsequently, the system temperature was lowered to room temperature, filtered, and the filtered product was washed and dried to obtain a modified flame retardant.
[0015] In the above reaction process, in a trimethylbenzene and dioxane system, an acidic medium is used to allow the aldehyde group on 1,3,5-triformylphloroglucinol and the amino group on p-phenylenediamine to undergo a Schiff base reaction to form an amide structure, which is then reacted with 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide through a phosphine-hydrogen addition reaction to prepare a flame retardant.
[0016] Furthermore, the mass ratio of 1,3,5-triformylphloroglucinol to p-phenylenediamine is (60-65):(60-63).
[0017] Further, the fireproof layer is prepared by the following steps:
[0018] The modified flame retardant, polyether polyol, catalyst dibutyltin dilaurate, silicone oil, Tween 80 and deionized water were stirred at room temperature at a rate of 1200 rpm for ten minutes, and then isocyanate was added and stirred for 1 minute. Then, the mixture was placed in a mold for foaming, and then the system was placed at a constant temperature of 60°C for aging for 5 hours to obtain a fireproof layer.
[0019] Furthermore, the mass ratio of the modified flame retardant, 100 parts of polyether polyol, dibutyltin dilaurate, silicone oil AK8006, Tween 80, deionized water and isocyanate is (0.1-1.0):100:(0.2-0.23-0.3):(5-5.6-6):(0.5-0.73-1)::(0.3-0.34-0.4):14.
[0020] Furthermore, in step S3, the specific operation of performing hydrophobic treatment on the silk fibroin fiber is as follows:
[0021] A1. Collect silk, wash it with deionized water, then drain the water, cut it into pieces, and obtain silk fibers; mix urea and guanidine hydrochloride in a mass ratio of 2:1 to obtain a degumming solution; place the silk fibers in the degumming solution at a bath ratio of 1g:20mL, stir until uniform, and then increase the system temperature to 100°C. After treating for 24 hours, add 100mL of deionized water to terminate the reaction, cool the system to room temperature, filter, wash the filtered material with deionized water, and then dry to obtain silk fibroin fibers;
[0022] A2. Add silk fibroin fiber to deionized water, use NaOH alkaline solution to adjust the pH value of the system to 8, add acetic anhydride after stirring evenly, continue stirring until the pH value of the system stabilizes at 8, and then continue to react for 1 hour, then use 1 mol / L hydrochloric acid solution to adjust the pH value of the system to 7, filter, wash the filtrate with deionized water, and dialyze the filtrate at 4°C for 48 hours to remove residual acetic anhydride, and mix it with the filtrate after drying to obtain hydrophobic treated silk fibroin fiber.
[0023] During the above reaction process, the amino group on the silk fibroin fiber attacks the carbon atom on the anhydride carbonyl group to undergo nucleophilic substitution. As the degree of acetylation increases, the acylation reaction introduces hydrophobic acetyl groups, exposing a large number of hydrophobic groups originally located inside, thereby increasing the hydrophobicity of the material.
[0024] Furthermore, in step A2, the mass ratio of silk fibroin to acetic anhydride is 1:(0.1-0.3).
[0025] Further, carboxylated expanded graphite is prepared by the following steps:
[0026] B1. Wash the flake graphite with deionized water, dry it naturally in the sun, then add it to a reactor, add a strong acid layer intercalant and an oxidant, stir evenly, raise the system temperature to 40-60°C, react for 2 hours, and filter to obtain expanded graphite;
[0027] B2, after the expanded graphite is placed in a 12wt% hydrazine hydrate solution and stirred evenly, the system temperature is raised to treat for 1 hour, then the system is cooled to room temperature, filtered and resuspended in a 0.3-0.5mol / L hydrochloric acid solution, the system temperature is raised to 60°C, and after two hours of treatment, carboxylated expanded graphite is obtained;
[0028] In the above reaction process, graphite is first mixed with a strong acid and an oxidant, and heated for oxidation reaction. Under the action of the oxidant, the graphite is oxidized to convert the neutral network macromolecules of the graphite layer into planar macromolecules with positive charges. Due to the repulsion of like positive charges, the distance between graphite layers increases, so that expanded graphite is generated during the heating process, and the functional groups in the graphite are oxidized to contain carbonyl groups. Subsequently, hydrazine hydrate is used as a reducing agent for reduction reaction to reduce the carbonyl groups in the oxidized graphite to hydroxyl groups, and then the hydroxyl groups are hydrolyzed to obtain carboxyl groups.
[0029] Further, the fiber-based gel is prepared by the following steps:
[0030] C1, add 0.1 mol / L 2-morpholineethanesulfonic acid and 0.05 mol / L NaCl to 30 mL sterile deionized water, and use NaOH solution to adjust the pH value of the system to 5.1 to obtain 2-morpholineethanesulfonic acid buffer for standby use;
[0031] C2, dissolving carboxylated expanded graphite, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and dopamine hydrochloride in 20 mL of 2-morpholineethanesulfonic acid buffer, and fully stirring for 24 hours at room temperature under an inert gas atmosphere to obtain modified carboxylated expanded graphite;
[0032] C3. Add hydrophobic treated silk fibroin fibers and modified carboxylated expanded graphite into deionized water and perform ultrasonic treatment at a power of 400 W for 2 hours to obtain a fiber-based gel.
[0033] In the above reaction process, the modified carboxylated expanded graphite carries carboxyl groups, and the carboxyl groups and the amino groups on dopamine hydrochloride are reacted to form amide bonds using an EDC / NHS system in a 2-morpholineethanesulfonic acid solution, thereby grafting the catechol structure onto the graphite surface. Subsequently, the hydrophobically treated silk fibroin fibers are ultrasonically treated in deionized water, and cross-linking occurs between the silk fibroin fibers and the amide bonds to form a gel system. In the subsequent process, catechol can promote the cross-linking of the gel by Michael addition with active amines and alkylthioates in the protein.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] In the technical solution of the present invention, firstly, in a trimethylbenzene and dioxane system, through an acidic medium, the aldehyde group on 1,3,5-triformyl phloroglucinol and the amino group on p-phenylenediamine undergo Schiff base reaction to form an amide structure. Then, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is reacted by phosphorus hydrogen addition to prepare a flame retardant. Compared with inorganic flame retardants, the addition in polyurethane materials does not lead to a decrease in its mechanical properties. For traditional 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide flame retardants, a higher residual carbon rate can be obtained, which is conducive to forming a dense carbon layer to prevent internal thermal decomposition products from entering the gas phase and continuing to participate in combustion, and has a better flame retardant effect. Subsequently, the obtained flame retardant is added to polyurethane for co-foaming to prepare a polyurethane material with flame retardant effect as a fireproof layer.
[0036] The silk fibroin fiber is subjected to hydrophobic treatment and then mixed with dopamine-modified carboxylated expanded graphite to prepare a fiber-based gel. The amino group on the silk fibroin fiber attacks the carbon atom on the anhydride carbonyl group to cause nucleophilic substitution. As the degree of acetylation increases, the acylation reaction introduces a hydrophobic acetyl group, and the hydrophobic groups originally inside are exposed in large quantities, which increases the hydrophobicity of the material. Then, expanded graphite is prepared, followed by carboxylation treatment, and then modified with dopamine. The modified graphene can form intermolecular hydrogen bonds with the silk fibroin fiber, and the silk fibroin fiber can self-crosslink to form a gel system. The gel is coated on the surface of the fireproof layer, and then a layer of oxidizing solution is sprayed, and then the fireproof layer is used to sandwich the fiber-based gel in the middle, pressure is applied, fixed, and then the material is freeze-dried to form a fireproof layer-gel layer-fireproof layer structure. After coating with an oxidizing solution, some of the catechol groups are oxidized into quinones, which can form covalent bonds with the thioalkyl and amino groups in the protein fibers through Michael addition, thereby improving the gel strength and promoting the adhesion between the gel and the polyurethane system at the interface after freeze-drying, preventing debonding. The gel has good thermal insulation and fire-resistant effects after freeze-drying. DETAILED DESCRIPTION
[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] The reagents used in the following examples and comparative examples are all of analytical grade. The polyether polyol is provided by Guangzhou Qihua Chemical Co., Ltd., model LY4110.
[0039] Example 1
[0040] The modified flame retardant is prepared by the following steps:
[0041] Trimethylbenzene and dioxane were mixed in a volume ratio of 1:1, stirred evenly, 60 mg of 1,3,5-triformylphloroglucinol and 60 mg of p-phenylenediamine were added, and stirring was continued until uniform. Then 0.5 mL of 3 mol / L acetic acid solution was added, and the system temperature was increased to 50-90°C. After reacting for 8 hours, 2.5 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, and the reaction was continued for 24 hours. Then, the system temperature was lowered to room temperature, filtered, and the filtered product was washed and dried to obtain a modified flame retardant.
[0042] Example 2
[0043] The difference between this embodiment and embodiment 1 is that the amount of 1,3,5-triformylphloroglucinol used is 63 mg, the amount of p-phenylenediamine used is 61 mg, and the amount of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide used is 3.1 g.
[0044] Example 3
[0045] The difference between this embodiment and embodiment 1 is that the amount of 1,3,5-triformylphloroglucinol used is 65 mg, the amount of p-phenylenediamine used is 63 mg, and the amount of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide used is 3.5 g.
[0046] Example 4
[0047] The hydrophobic treated silk fibroin fiber is prepared by the following steps:
[0048] A1. Collect silk, wash it with deionized water, then drain the water, cut it into pieces, and obtain silk fibers; mix urea and guanidine hydrochloride in a mass ratio of 2:1 to obtain a degumming solution; place the silk fibers in the degumming solution at a bath ratio of 1g:20mL, stir until uniform, and then increase the system temperature to 100°C. After treating for 24 hours, add 100mL of deionized water to terminate the reaction, cool the system to room temperature, filter, wash the filtered material with deionized water, and then dry to obtain silk fibroin fibers;
[0049] A2. Add 10 g of silk fibroin fiber into deionized water, adjust the pH value of the system to 8 with NaOH solution, stir evenly and add 1-3 g of acetic anhydride, continue stirring until the pH value of the system stabilizes at 8 and then continue to react for 1 hour, then use 1 mol / L hydrochloric acid solution to adjust the pH value of the system to 7, filter and wash the filtrate with deionized water, and dialyze the filtrate at 4°C for 48 hours to remove residual acetic anhydride, dry and mix with the filtrate to obtain hydrophobically treated silk fibroin fiber.
[0050] Example 5
[0051] The difference between this embodiment and embodiment 4 is that in step A2, the amount of acetic anhydride used is 2 g.
[0052] Example 6
[0053] The difference between this embodiment and embodiment 4 is that in step A2, the amount of acetic anhydride used is 3 g.
[0054] Example 7
[0055] Carboxylated expanded graphite is prepared by the following steps:
[0056] B1. Wash the flake graphite with deionized water, dry it naturally in the sun, then add it to a reactor, add a strong acid layer intercalant and an oxidant, stir evenly, raise the system temperature to 40-60°C, react for 2 hours, and filter to obtain expanded graphite;
[0057] B2. After the expanded graphite is placed in a 12wt% hydrazine hydrate solution and stirred evenly, the system temperature is raised to treat for 1 hour, then the mixture is cooled to room temperature, filtered and resuspended in a 0.3-0.5mol / L hydrochloric acid solution, the system temperature is raised to 60°C, and after treating for two hours, carboxylated expanded graphite is obtained.
[0058] Example 8
[0059] A method for preparing a thermal insulation and fireproof composite material for construction, comprising the following steps:
[0060] S1, 0.1 parts of the modified flame retardant prepared in Example 1, 100 parts of polyether polyol, 0.2 parts of catalyst dibutyltin dilaurate, 5 parts of silicone oil AK8006, 0.5 parts of Tween 80 and 0.3 parts of deionized water were stirred at room temperature at a rate of 1200 rpm for ten minutes, and then 140 parts of isocyanate PM-200 were added, and stirring was continued for 1 minute, and then placed in a mold for foaming, and then the system was placed at 60°C for constant temperature aging for 5 hours to obtain a fireproof layer;
[0061] S2, 0.585g 0.1mol / L 2-morpholineethanesulfonic acid and 0.0876g 0.05mol / L NaCl were added to 30mL sterile deionized water, and the pH value of the system was adjusted to 5.1 using NaOH solution to obtain 2-morpholineethanesulfonic acid buffer for standby use; 10g carboxylated expanded graphite, 0.192g 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, 0.115g N-hydroxysuccinimide and 0.5g dopamine hydrochloride were dissolved in 20mL 2-morpholineethanesulfonic acid buffer, and stirred for 24 hours at room temperature and inert gas atmosphere to obtain modified carboxylated expanded graphite; 6mg of the hydrophobic treated silk fibroin fiber prepared in Example 4 and 5mg of the modified carboxylated expanded graphite prepared in Example 7 were added to deionized water, and ultrasonically treated for 2 hours at a power of 400W to obtain a fiber-based gel;
[0062] S3. Coat the fiber-based gel on the surface of the fireproof layer prepared in step S1, then spray a layer of 0.4 mol / L sodium periodate solution according to the standard of 1 mL / cm2, and then use the fireproof layer to sandwich the fiber-based gel prepared in step S2 in the middle, apply a pressure of 10% d / L strain, fix for 1 hour, and then freeze-dry the material to form a fireproof layer-gel layer-fireproof layer structure, thereby obtaining a thermal insulation and fireproof composite material for construction.
[0063] Example 9
[0064] The difference between this embodiment and Example 8 is that in step S1, the modified flame retardant is prepared in Example 2, and the mass ratio of the modified flame retardant, polyether polyol, dibutyltin dilaurate, silicone oil AK8006, Tween 80, deionized water and isocyanate PM-200 is 0.5:100:0.23:5.6:0.73:0.34:140; in step S2, the amount of dopamine hydrochloride used is 1.5 g, the hydrophobic treated silk fibroin fiber is prepared in Example 5, and the amount of modified carboxylated expanded graphite used is 8 mg.
[0065] Example 10
[0066] The difference between this embodiment and Example 8 is that in step S1, the modified flame retardant is prepared in Example 3, and the mass ratio of the modified flame retardant, polyether polyol, dibutyltin dilaurate, silicone oil AK8006, Tween 80, deionized water and isocyanate PM-200 is 1.0:100:0.3:6:1:0.4:140; in step S2, the amount of dopamine hydrochloride used is 2 g, the hydrophobic treated silk fibroin fiber is prepared in Example 6, and the amount of modified carboxylated expanded graphite used is 10 mg.
[0067] Comparative Example 1
[0068] The difference between this comparative example and Example 9 is that no silk fibroin fiber is added.
[0069] Comparative Example 2
[0070] The difference between this comparative example and Example 9 is that the silk fibroin fibers are not hydrophobically modified.
[0071] Comparative Example 3
[0072] The difference between this comparative example and Example 9 is that no carboxylated expanded graphite is added.
[0073] Comparative Example 4
[0074] The difference between this comparative example and Example 9 is that the carboxylated expanded graphite is not modified with dopamine.
[0075] Comparative Example 5
[0076] The difference between this comparative example and Example 9 is that no modified flame retardant is added to the polyurethane.
[0077] The flame retardant effect of the composite materials prepared in Examples 8-10 and Comparative Examples 1-5 is now tested. The samples are made into square strips with a length of 10 cm and a width of 2 cm. 15 strips of each sample are taken. Under the conditions of an ambient temperature of 10-35°C, a relative humidity of 45%-75% and an air oxygen concentration of 16%-27%, the sample is ignited from the top. After confirming that the top of the sample is completely on fire, the igniter is immediately removed, and the burning time and the burning length of the sample are recorded. When igniting the sample, the longest time for the flame to act is 30 seconds. If it cannot be ignited within 30 seconds, the oxygen concentration is increased and the ignition is continued until it is ignited within 30 seconds. Each sample is tested 15 times and the average value is taken. The test results are shown in Table 1 below.
[0078] Table 1 Test of flame retardant effect of composite materials prepared in Examples 8-10 and Comparative Examples 1-5
[0079] project Burning time(s) Burning length (cm) Example 8 0.9 1.6 Example 9 0.8 1.5 Example 10 0.9 1.6 Comparative Example 1 1.3 1.9 Comparative Example 2 1.0 1.7 Comparative Example 3 1.5 2.0 Comparative Example 4 1.5 2.0 Comparative Example 5 3.1 6.1
[0080] As shown in Table 1 above, the composite material obtained in Example 9 has the best flame retardant effect. As shown in the results of Comparative Examples 1 and 2, the silk fibroin fiber molecules contain a large amount of amino acids and polypeptides, which can be decomposed at high temperatures to produce a large amount of inactive gases, thereby reducing the concentration of oxygen and combustible gases during combustion and inhibiting the spread of flames. The modified silk fibroin fiber contains acetyl groups, which have a good mixing effect with the gel system and are evenly dispersed in the system to improve its flame retardant effect. As shown in the results of Comparative Examples 3 and 4, expanded graphite can form a carbon layer during combustion to inhibit flames.
[0081] The thermal insulation effect of the composite materials prepared in Examples 8-10 and Comparative Examples 1-5 is now tested. The thermal conductivity of the thermal insulation material is measured at room temperature by the transient plane heat source method to determine the thermal insulation effect of the material. Five readings are obtained for each sample and the average value is taken. The test results are shown in Table 2.
[0082] Table 2 Thermal insulation effect test of composite materials prepared in Examples 8-10 and Comparative Examples 1-5
[0083] project Thermal conductivity (W / m / K) Example 8 0.0230 Example 9 0.0225 Example 10 0.0227 Comparative Example 1 0.0301 Comparative Example 2 0.0307 Comparative Example 3 0.0415 Comparative Example 4 0.0351 Comparative Example 5 0.0459
[0084] From the results in Table 2, it can be seen that the composite materials prepared in Examples 8-10 all have lower thermal conductivity and better thermal insulation effect. From the results in the comparative example, it can be seen that adding silk fibroin fiber-modified expanded graphite aerogel can improve the thermal insulation effect of the composite material.
[0085] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0086] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a thermal insulation and fireproof composite material for construction, characterized in that: The following steps are involved: S1. Modifying 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide using 1,3,5-triformylphloroglucinol and p-phenylenediamine to obtain a modified flame retardant; S2. Adding a modified flame retardant to the polyurethane material to prepare a fireproof layer; S3, hydrophobic treatment of silk fibroin fibers, followed by mixing with dopamine-modified carboxylated expanded graphite to prepare a fiber-based gel; S4. Coat the fiber-based gel on the surface of the fireproof layer, then spray a layer of oxidizing solution, and then use the fireproof layer to sandwich the fiber-based gel in the middle, apply pressure, fix, and then freeze-dry the material to form a fireproof layer-gel layer-fireproof layer structure, thereby obtaining a thermal insulation and fireproof composite material for construction.
2. The method for preparing a thermal insulation and fireproof composite material for construction according to claim 1, characterized in that: In step S1, the modified flame retardant is prepared by the following steps: The trimethylbenzene and dioxane were mixed in a volume ratio of 1:1, and 1,3,5-triformylphloroglucinol and p-phenylenediamine were added after stirring evenly. The acetic acid solution was added after continuing to stir until evenly mixed. The system temperature was raised to 50-90°C, and after reacting for 8 hours, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, and the reaction was continued for 24 hours. Subsequently, the system temperature was lowered to room temperature, filtered, and the filtered product was washed and dried to obtain a modified flame retardant.
3. The method for preparing a thermal insulation and fireproof composite material for construction according to claim 2, characterized in that: The mass ratio of 1,3,5-triformylphloroglucinol to p-phenylenediamine is (60-65):(60-63).
4. The method for preparing a thermal insulation and fireproof composite material for construction according to claim 1, characterized in that: The fireproof layer is prepared by the following steps: The modified flame retardant, polyether polyol, catalyst dibutyltin dilaurate, silicone oil, Tween 80 and deionized water are stirred, and then isocyanate is added, and stirring is continued. Then, the mixture is placed in a mold for foaming and then the system is placed at a constant temperature of 60° C. for aging for 5 hours to obtain a fireproof layer.
5. The method for preparing a thermal insulation and fireproof composite material for construction according to claim 4, characterized in that: The mass ratio of modified flame retardant, polyether polyol, catalyst dibutyltin dilaurate, silicone oil, Tween 80, deionized water and isocyanate is (0.1-1.0):100:(0.2-0.23-0.3):(5-5.6-6):(0.5-0.73-1)::(0.3-0.34-0.4):
14.
6. The method for preparing a thermal insulation and fireproof composite material for construction according to claim 1, characterized in that: In step S3, the specific operation of hydrophobic treatment of silk fibroin fibers is as follows: A1. Collect silk, wash it, drain the water, cut it into pieces, and obtain silk fiber; mix urea and guanidine hydrochloride in a mass ratio of 2:1 to obtain a degumming solution; place the silk fiber in the degumming solution at a bath ratio of 1g:20mL, stir until uniform, and then increase the system temperature to 100°C. After treating for 24 hours, add deionized water to terminate the reaction, cool the system to room temperature, filter, wash the filtered material with deionized water, and then dry it to obtain silk fibroin fiber; A2. Add silk fibroin fiber to deionized water, adjust the pH value of the system to 8, add acetic anhydride after stirring evenly, continue stirring until the pH value of the system stabilizes at 8, and then continue to react for 1 hour, then adjust the pH value of the system to 7, filter, wash the filtrate, and dialyze the filtrate at 4°C for 48 hours, dry it, and mix it with the filtrate to obtain hydrophobically treated silk fibroin fiber.
7. The method for preparing a thermal insulation and fireproof composite material for construction according to claim 6, characterized in that: In step A2, the mass ratio of silk fibroin to acetic anhydride is 1:(0.1-0.3).
8. The method for preparing a thermal insulation and fireproof composite material for construction according to claim 1, characterized in that: The carboxylated expanded graphite is prepared by the following steps: B1. Wash the flake graphite with deionized water, dry it, and then add it to a reactor, add a strong acid layer intercalant and an oxidant, stir evenly, raise the system temperature to 40-60° C., react for 2 hours, and filter to obtain expanded graphite; B2. Place the expanded graphite in a hydrazine hydrate solution and stir evenly, then raise the system temperature to treat for 1 hour, then return to room temperature, filter and resuspend in a hydrochloric acid solution, raise the system temperature to 60°C, and treat for two hours to obtain carboxylated expanded graphite.
9. The method for preparing a thermal insulation and fireproof composite material for construction according to claim 1, characterized in that: The fiber-based gel is prepared by the following steps: C1, add 2-morpholineethanesulfonic acid and NaCl into sterile deionized water, use NaOH solution to adjust the pH value of the system to 5.1, and obtain 2-morpholineethanesulfonic acid buffer for standby use; C2, dissolving carboxylated expanded graphite, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and dopamine hydrochloride in 2-morpholineethanesulfonic acid buffer, and fully stirring for 24 hours at room temperature under an inert gas atmosphere to obtain modified carboxylated expanded graphite; C3. Add hydrophobic treated silk fibroin fibers and modified carboxylated expanded graphite into deionized water and perform ultrasonic treatment for 2 hours to obtain a fiber-based gel.
10. A composite material obtained by the method for preparing a thermal insulation and fireproof composite material for construction as claimed in any one of claims 1 to 9.
Citation Information
Cited By
Preparation process of polyurethane nanoscale microporous membrane for protective clothing
CN119613802A
Preparation Process of Polyurethane Nanoscale Microporous Membrane for Protective Clothing
CN119613802B
Preparation process of composite current collector
CN119955157A