Semiconductor device and manufacturing method thereof

By forming through grooves in the MEMS device and removing the interface layer, combining the filling layer and the release hole to remove the sacrificial layer, the device failure problem caused by interface layer corrosion is solved, and the overall structure and production efficiency of the device are improved.

CN118929563APending Publication Date: 2024-11-12RUNXIN SENSING TECHNOLOGY (NANCHANG) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310538464.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When removing the sacrificial layer of existing MEMS devices, the interface layer between the sensitive material layer and the side wall layer is easily corroded, resulting in device failure, and the process of removing the interface layer has problems such as high cost and limited production capacity.

Method used

By forming a through groove on the sensitive material layer and removing the interface layer at the bottom of the groove, and then forming a fill layer between the side wall layer and the sensitive material layer, the sacrificial layer is removed using the release hole to form a cavity structure to avoid the interface layer Cracking caused by corrosion.

Benefits of technology

The overall structure of semiconductor devices is enhanced, device failure caused by corrosion of the interface layer is avoided, production costs are reduced and production capacity is increased.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929563A_ABST
    Figure CN118929563A_ABST
Patent Text Reader

Abstract

The invention discloses a semiconductor device and a manufacturing method thereof. The method comprises the following steps: providing a sensitive material layer; a sacrificial layer and a side wall layer surrounding the sacrificial layer are formed on the second surface of the sensitive material layer, release holes connected with the sacrificial layer are formed in the top of the side wall layer, and an interface layer is formed between the bottom of the side wall layer and the second surface of the sensitive material layer; the sensitive material layer is etched from the first surface of the sensitive material layer to form a groove penetrating through the sensitive material layer, the opening position of the groove is opposite to the bottom of the side wall layer, and the bottom of the groove is exposed out of the interface layer; removing the interface layer exposed at the bottom of the groove; forming a filling layer for filling the groove; and removing the sacrificial layer through the release hole so as to form a cavity structure between the side wall layer and the sensitive material layer. The interface layer between the sensitive material layer and the side wall layer is removed through the groove penetrating through the sensitive material layer, and cracking between the sensitive material layer and the side wall layer due to transverse corrosion of the interface layer is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a semiconductor device and a method for manufacturing the same. Background Art

[0002] MEMS (Micro-Electro-Mechanical System) refers to a micro system that integrates mechanical components, drive components, optical systems, and electronic control systems into a whole. MEMS devices have advantages such as small size and low power consumption, and have a wide range of application scenarios in smart phones, tablets, game consoles, automobiles, drones, and other fields. Similar to integrated circuits, MEMS devices are also developing in the direction of high performance, miniaturization, low cost, and integration.

[0003] The cavity structure of existing MEMS devices is formed by removing the sacrificial layer between the sensitive material layer and the sidewall layer through the release hole using a wet or dry etching process. However, there is usually an interface layer between the sensitive material layer and the sidewall layer. When removing the sacrificial layer, the etching reaction gas or liquid will corrode the interface layer, causing cracks in the sensitive material layer and the sidewall layer, resulting in serious process problems and causing device failure. Summary of the invention

[0004] A series of simplified concepts are introduced in the Summary of the Invention, which will be further described in detail in the Detailed Description of the Invention. The Summary of the Invention does not mean to attempt to define the key features and essential technical features of the claimed technical solution, nor does it mean to attempt to determine the scope of protection of the claimed technical solution.

[0005] In view of the existing problems, an embodiment of the present invention provides a method for manufacturing a semiconductor device, the method comprising:

[0006] Providing a sensitive material layer, the sensitive material layer comprising a first surface and a second surface opposite to the first surface;

[0007] A sacrificial layer and a sidewall layer surrounding the sacrificial layer are formed on the second surface of the sensitive material layer, a release hole connected to the sacrificial layer is formed on the top of the sidewall layer, and an interface layer is formed between the bottom of the sidewall layer and the second surface of the sensitive material layer;

[0008] Etching the sensitive material layer from the first surface of the sensitive material layer to form a groove penetrating the sensitive material layer, wherein the opening position of the groove is arranged opposite to the bottom of the sidewall layer, and the bottom of the groove exposes the interface layer;

[0009] removing the interface layer exposed at the bottom of the groove;

[0010] forming a filling layer filling the groove;

[0011] The sacrificial layer is removed through the release hole to form a cavity structure between the sidewall layer and the sensitive material layer.

[0012] In one embodiment, removing the interface layer exposed at the bottom of the groove includes:

[0013] The interface layer is physically bombarded to remove the interface layer.

[0014] In one embodiment, removing the interface layer exposed at the bottom of the groove includes:

[0015] The interface layer is reduced by using a reducing agent to remove the interface layer.

[0016] In one embodiment, forming a filling layer filling the groove includes:

[0017] The filling layer material is deposited under vacuum conditions to form the filling layer.

[0018] In one embodiment, the filling layer material is a material that is more difficult to oxidize than the sensitive material layer.

[0019] In one embodiment, the width of the groove is smaller than the width of the bottom of the sidewall layer.

[0020] In one embodiment, providing the sensitive material layer comprises: providing a first substrate, and forming the sensitive material layer on the first substrate, wherein the first surface of the sensitive material layer is disposed on the first substrate;

[0021] Before forming the groove, the method further includes: forming a second substrate on top of the sidewall layer;

[0022] The first substrate is removed to expose the first surface of the sensitive material layer.

[0023] In one embodiment, after forming the filling layer, the method further comprises: forming a third substrate on the first surface of the sensitive material layer;

[0024] The second substrate is removed to expose the release hole.

[0025] In one embodiment, the sensitive material layer includes a piezoelectric layer, a first electrode is formed on the first surface of the sensitive material layer, and a second electrode is formed on the second surface of the sensitive material layer.

[0026] Another aspect of an embodiment of the present invention provides a semiconductor device, the semiconductor device comprising:

[0027] a sensitive material layer, the sensitive material layer comprising a first surface and a second surface opposite to the first surface;

[0028] a sidewall layer formed on the second surface of the sensitive material layer;

[0029] A groove extending from the first surface of the sensitive material layer through the sensitive material layer, wherein the opening position of the groove is arranged opposite to the bottom of the sidewall layer, the groove is filled with a filling layer, and the bottom of the filling layer is connected to the bottom of the sidewall layer;

[0030] A cavity structure is arranged between the sidewall layer and the sensitive material layer.

[0031] According to the semiconductor device manufacturing method and semiconductor device provided by the embodiment of the present invention, by forming a groove penetrating the sensitive material layer and removing the interface layer through the groove, it is possible to avoid cracking between the sidewall layer and the sensitive material layer due to corrosion of the interface layer, thereby enhancing the overall structure of the semiconductor device. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The following drawings of the present invention are used to understand the present invention as part of the present invention. The embodiments of the present invention are shown in the drawings and the description thereof is used to explain the principle of the present invention.

[0033] In the attached figure:

[0034] Figures 1A to 1C A cross-sectional schematic diagram of a semiconductor device obtained by sequentially implementing each step according to an existing method for manufacturing a semiconductor device is shown;

[0035] Figure 2 A schematic flow chart showing a method for manufacturing a semiconductor device according to a specific embodiment of the present invention;

[0036] FIG. 3A to FIG. 3E The cross-sectional view of a semiconductor device obtained by sequentially performing various steps in a method for manufacturing a semiconductor device according to an embodiment of the present invention is shown. DETAILED DESCRIPTION

[0037] In the following description, a large number of specific details are provided to provide a more thorough understanding of the present invention. However, it is apparent to those skilled in the art that the present invention can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present invention, some technical features well known in the art are not described.

[0038] It should be understood that the present invention can be implemented in different forms and should not be construed as being limited to the embodiments presented herein. On the contrary, providing these embodiments will make the disclosure thorough and complete and fully convey the scope of the present invention to those skilled in the art. In the accompanying drawings, the sizes and relative sizes of layers and regions may be exaggerated for clarity. The same reference numerals throughout represent the same elements.

[0039] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there are no intervening elements or layers. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present invention, the first element, component, region, layer or part discussed below can be represented as a second element, component, region, layer or part.

[0040] Spatially relative terms such as "under", "beneath", "below", "under", "above", "above", etc., may be used here for convenience of description to describe the relationship between an element or feature shown in the figure and other elements or features. It should be understood that in addition to the orientation shown in the figure, the spatial relationship terms are intended to also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is turned over, then the elements or features described as "under other elements" or "under it" or "under it" will be oriented as "on" other elements or features. Therefore, the exemplary terms "under" and "under" may include both upper and lower orientations. The device can be oriented otherwise (rotated 90 degrees or other orientations) and the spatial descriptors used herein are interpreted accordingly.

[0041] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be limiting of the present invention. When used herein, the singular forms "one", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.

[0042] like Figure 1A-Figure 1C As shown, in the current manufacturing method of semiconductor devices, in order to obtain a cavity structure, it is first necessary to form a sacrificial layer 103 surrounded by a sidewall layer 102 on the sensitive material layer 101, wherein the sidewall layer 102 and the sacrificial layer 103 have a higher etching selectivity ratio; then, a wet or dry process is used to remove the sacrificial layer 103 through a release hole 104 formed in the sidewall layer 102, thereby forming a cavity structure 106 surrounded by the sidewall layer 102.

[0043] However, there is usually an interface layer 105 between the sensitive material layer 101 and the sidewall layer 102. The interface layer is generally formed by oxidation of the surface of the sensitive material layer 101 when the sidewall layer 102 is formed, and is relatively difficult to remove. When removing the sacrificial layer 103, the etching reaction gas or liquid will react with the interface layer 105, causing the interface layer 105 to be etched away, thereby causing the sensitive material layer 101 and the sidewall layer 102 connected by the interface layer 105 to crack, resulting in serious process problems and causing device failure.

[0044] The main reason why the interface layer 105 is corroded from the side during the process of releasing the sacrificial layer 103 is that the interface layer 105 and the sacrificial layer 103 are made of the same or similar materials, and the etchant used to remove the sacrificial layer 103 will also react with the interface layer 105. If an etchant that is not prone to damaging the interface layer 105 is used to remove the sacrificial layer 103, it will take a long time to release the sacrificial layer 103, resulting in high costs and limited mass production capacity.

[0045] In response to the above problems, Figure 2 As shown, the embodiment of the present invention provides a method 200 for manufacturing a semiconductor device, comprising the following steps:

[0046] Step S210: providing a sensitive material layer, wherein the sensitive material layer comprises a first surface and a second surface opposite to the first surface;

[0047] Step S220: forming a sacrificial layer and a sidewall layer surrounding the sacrificial layer on the second surface of the sensitive material layer, wherein a release hole connected to the sacrificial layer is formed on the top of the sidewall layer, and an interface layer is formed between the bottom of the sidewall layer and the second surface of the sensitive material layer;

[0048] Step S230: etching the sensitive material layer from the first surface of the sensitive material layer to form a groove penetrating the sensitive material layer, wherein the opening position of the groove is arranged opposite to the bottom of the sidewall layer, and the bottom of the groove exposes the interface layer;

[0049] Step S240: removing the interface layer exposed at the bottom of the groove;

[0050] Step S250: forming a filling layer filling the groove;

[0051] Step S260: removing the sacrificial layer through the release hole to form a cavity structure between the sidewall layer and the sensitive material layer.

[0052] The method 200 for manufacturing a semiconductor device according to an embodiment of the present invention can avoid cracking between the sidewall layer and the sensitive material layer due to corrosion of the interface layer by forming a groove penetrating the sensitive material layer and removing the interface layer through the groove, thereby enhancing the overall structure of the semiconductor device.

[0053] In order to fully understand the present invention, detailed structures and steps will be presented in the following description to illustrate the technical solutions proposed by the present invention. The preferred embodiments of the present invention are described in detail below, but in addition to these detailed descriptions, the present invention may also have other implementations.

[0054] Combine the following Figure 3A to Figure 3E The implementation process of a method for manufacturing a semiconductor device according to an embodiment of the present invention is described exemplarily. Figure 3A to Figure 3E The cross-sectional view of a semiconductor device obtained by sequentially performing various steps in a method for manufacturing a semiconductor device according to an embodiment of the present invention is shown.

[0055] First, step S210 is performed to provide a sensitive material layer, where the sensitive material layer includes a first surface and a second surface opposite to the first surface.

[0056] For example, Figure 3AAs shown, a first substrate (not shown) is provided, and a sensitive material layer 301 is formed on the first substrate. The sensitive material layer 301 includes a first surface and a second surface opposite to the first surface, and the first surface is arranged on the first substrate. The first substrate can be any suitable semiconductor substrate, such as a bulk silicon substrate, and can also be at least one of the following materials: Si, Ge, SiGe, SiC, SiGeC, InAs, GaAs, InP or other III / V compound semiconductors, and also includes a multilayer structure composed of these semiconductors, or silicon on insulator (SOI), stacked silicon on insulator (SSOI), stacked silicon germanium on insulator (S-SiGeOI), silicon germanium on insulator (SiGeOI) and germanium on insulator (GeOI), or can also be double-side polished silicon wafers (Double Side Polished Wafers, DSP), or can also be ceramic substrates such as aluminum oxide, quartz or glass substrates, etc.

[0057] Exemplarily, before forming the sensitive material layer 301 on the first substrate, the surface of the first substrate is first oxidized to form an oxide layer. After the oxide layer is formed, a first electrode (not shown) may also be formed on the first substrate. In one example, the method for forming the first electrode includes: depositing a first electrode material layer to cover the first substrate, then forming a patterned mask layer on the first electrode material layer, the mask layer defining a pattern of the first electrode, then etching the first electrode material layer using the patterned mask layer as a mask to form the first electrode, and finally removing the patterned mask layer.

[0058] In another example, a lift-off process may be used to form the first electrode, that is, a patterned mask layer is first formed on the surface of the first substrate, and then a first electrode material layer covering the patterned mask layer is formed, and finally the patterned mask layer is lifted off and the first electrode material layer above it is removed to obtain the first electrode.

[0059] The material of the first electrode may be a conductive material or a semiconductor material, wherein the conductive material may be a metal material having conductive properties, and the metal material may be a metal such as aluminum (Al), copper (Cu), gold (Au), platinum (Pt), or an alloy of metal and copper, etc. The semiconductor material may be Si, Ge, SiGe, SiC, SiGeC, etc.

[0060] Next, a sensitive material layer 301 is formed on the first substrate. The sensitive material layer 301 is used to realize the micro-electromechanical function of the semiconductor device, including but not limited to the piezoelectric layer. The piezoelectric layer generates voltage when subjected to external pressure. Conversely, if there is voltage on both sides of the piezoelectric layer, the piezoelectric layer will be slightly deformed. Based on the above characteristics of the piezoelectric layer, the mutual conversion between sound waves and electrical signals can be realized.

[0061] Exemplarily, a deposition method such as chemical vapor deposition, physical vapor deposition or atomic layer deposition can be used to deposit a piezoelectric material, and a metal element can be doped into the piezoelectric material to form a piezoelectric layer, and the doped metal element includes one or more of scandium, zirconium, calcium, titanium, magnesium, etc. Exemplarily, the material of the piezoelectric layer can specifically include aluminum nitride, lead zirconate titanate, zinc oxide, etc., and the embodiment of the present invention is not limited to this.

[0062] Continue to refer to Figure 3A After forming the sensitive material layer 301, a second electrode 302 may be formed on the sensitive material layer 301. When the sensitive material layer 301 is a piezoelectric layer, the first electrode, the piezoelectric layer, and the second electrode constitute a composite film, and the composite film may also include other film layers in addition to the above-mentioned film layers, which may be reasonably arranged according to the actual device, and is not specifically limited here.

[0063] In one example, the method for forming the second electrode 302 includes: depositing a second electrode material layer to cover the substrate, the second electrode material layer may be a metal material layer or a semiconductor material layer. Then, forming a patterned mask layer on the second electrode material layer, the mask layer defining a pattern of the second electrode, and then etching the second electrode material layer using the patterned mask layer as a mask to form the second electrode 302, and finally, removing the patterned mask layer.

[0064] In another example, a lift-off process may be used to form the second electrode 302, that is, a patterned mask layer is first formed on the surface of the substrate, and then a second electrode material layer covering the patterned mask layer is formed, and finally the patterned mask layer is lifted off and the second electrode material layer above it is removed to obtain a second electrode.

[0065] Next, step S220 is performed to form a sacrificial layer 303 and a sidewall layer 304 surrounding the sacrificial layer 303 on the sensitive material layer 301. A release hole connected to the sacrificial layer 303 is formed on the top of the sidewall layer 304, and an interface layer 306 is formed between the bottom of the sidewall layer 304 and the second surface of the sensitive material layer 301. The sidewall layer 304 is used to define the boundary of the cavity structure.

[0066] Exemplarily, a sacrificial layer 303 is first formed on the sensitive material layer 301, and a groove penetrating the sacrificial layer 303 is formed in the sacrificial layer 303, and the bottom of the groove exposes the second surface of the sensitive material layer 301. The deposition process used to deposit the sacrificial layer 303 includes chemical vapor deposition, physical vapor deposition, etc. After the sacrificial layer is deposited, a patterned photoresist layer is formed on the sacrificial layer 303, and the photoresist layer has a window defining the position of the groove. Thereafter, the sacrificial layer 303 is dry-etched using the photoresist layer as a mask to form a groove penetrating the sacrificial layer 303. The etching of the sacrificial layer 303 stops at the second surface of the sensitive material layer 301. After the etching of the sacrificial layer 303 is completed, the photoresist layer can be removed by a process such as photoresist ashing.

[0067] Next, a sidewall layer 304 is formed to fill the groove in the sacrificial layer and cover the surface of the sacrificial layer. That is, the sidewall layer 304 includes a portion formed in the groove and a portion covering the surface of the sacrificial layer 303. The sidewall layer 304 can be deposited by a deposition method such as chemical vapor deposition, physical vapor deposition or atomic layer deposition. There is a high etching selectivity between the sidewall layer 304 and the sacrificial layer 303, so that the sidewall layer 304 is not affected during the process of removing the sacrificial layer 303. For example, if the material of the sacrificial layer 303 is SiO2, polysilicon can be used as the material of the sidewall layer 304.

[0068] In some embodiments, a sidewall layer covering the sensitive material layer 301 may be formed first, a groove may be formed in the sidewall layer by etching, and then a sacrificial layer filling the groove may be formed. After that, the sacrificial layer above the sidewall layer may be removed by a chemical mechanical polishing process, and another portion of the sidewall layer covering the top of the sacrificial layer may be formed, so that the sidewall layer surrounds the sacrificial layer.

[0069] After forming the sidewall layer 304 surrounding the sacrificial layer 303, a release hole 305 connected to the sacrificial layer 303 is formed on the top of the sidewall layer 304. Specifically, the top of the sidewall layer 304 can be etched using the photoresist layer as a mask to form the release hole 305 above the sacrificial layer 303.

[0070] During the process of forming the sidewall layer 304 , the second surface of the sensitive material layer 301 exposed at the bottom of the trench in the sacrificial layer 303 is oxidized, thereby forming an interface layer 306 between the sensitive material layer 301 and the sidewall layer 304 . The interface layer 306 is an oxide layer and is usually difficult to remove.

[0071] Since the sensitive material layer 301 needs to be etched from the first surface of the sensitive material layer 301, the first substrate needs to be removed after the release hole 305 is formed to expose the first surface of the sensitive material layer 301. A second substrate can be bonded on the top of the sidewall layer 304 as a temporary substrate for carrying semiconductor devices; then, the first substrate is thinned to a certain thickness and then corroded to the oxide layer with an alkaline solution to remove the first substrate.

[0072] Next, step S230 is performed to etch the sensitive material layer 301 from the first surface of the sensitive material layer 301 to form a groove 307 penetrating the sensitive material layer 301 . The opening position of the groove 307 is arranged opposite to the bottom of the sidewall layer 304 , and the bottom of the groove 307 exposes the interface layer 306 .

[0073] Considering that if etching is performed downward from the top of the sidewall layer 304, the etching will be difficult due to the large thickness of the sidewall layer 304. Therefore, the embodiment of the present invention chooses to perform etching from the back side (i.e., the first surface) of the sensitive material layer 301 to form the groove 307. At this time, it is only necessary to etch through the sensitive material layer 301. The thickness of the sensitive material layer 301 is much smaller than the thickness of the sacrificial layer 303 and the sidewall layer 304. Therefore, when etching to form the groove 307, the required etching depth is small and the process difficulty is controllable.

[0074] In some embodiments, Figure 3B As shown, the width of the groove 307 remains unchanged from the opening downward, that is, the longitudinal section of the groove 307 is a rectangle. In this embodiment, a patterned photoresist layer can be formed on the first surface of the sensitive material layer 301, and the photoresist layer has an opening defining the position of the groove opening; then, the sensitive material layer 301 and the sidewall layer 304 are anisotropically etched using the photoresist layer as a mask, thereby forming a rectangular groove 307.

[0075] Furthermore, the width of the groove 307 is smaller than the width of the bottom of the sidewall layer 304, that is, the edge of the groove 307 is located within the range of the bottom of the sidewall layer 304, so that after the cavity structure is formed, the influence of the side corrosion of the interface layer on the anchor point position where the sensitive material layer 301 contacts the sidewall layer 304 is reduced.

[0076] In another embodiment, the width of the groove 307 gradually decreases from the opening downward, that is, the longitudinal cross-section of the groove 307 can be a triangle or a trapezoid. The formation of the groove 307 with a gradually decreasing width is conducive to reducing the influence of the groove 307 on the sidewall layer 304. As an implementation method, a polymer layer can be deposited on the sidewall of the groove during the etching of the sensitive material layer 301, so that the width of the groove gradually decreases from the opening downward. As another implementation method, a photoresist layer covering the first surface of the sensitive material layer 301 can be formed, and in the process of exposing the photoresist layer, a focus point is set above the center position of the photoresist layer to form a photoresist pattern with a thickness gradually decreasing from the outside to the inside at the opening position of the groove; based on the photoresist layer after exposure and development, the sensitive material layer and the sidewall layer are etched, so that the width of the groove 307 formed by etching gradually decreases from the opening downward. In another implementation, a photoresist layer can be formed to cover the first surface of the sensitive material layer 301; the photoresist layer is exposed and developed based on a grayscale photomask to form a photoresist pattern whose thickness gradually decreases from the outside to the inside at the opening position of the groove; the sensitive material layer 301 and the sidewall layer 304 are etched based on the exposed and developed photoresist layer to make the width of the groove 307 gradually decrease from the opening to the bottom.

[0077] Next, execute step S240, such as Figure 3C As shown, the interface layer 306 exposed at the bottom of the groove 307 is removed. The interface layer can be physically bombarded through the groove 307 to remove the interface layer 306 exposed at the bottom of the groove 307. Specifically, the interface layer 306 can be physically bombarded using plasma to remove the interface layer exposed at the bottom of the groove 307, so that the sidewall layer 304 is exposed at the bottom of the groove 307. Alternatively, the interface layer 306 can be reduced using a reducing agent to remove the interface layer 306. The reducing agent can be a reducing gas such as H2, or a reducing liquid.

[0078] Since the interface layer 306 is formed simultaneously between the sensitive material layer 301 and the sidewall layer 304 during the process of forming the sidewall layer 304, it is usually difficult to remove; for this reason, the embodiment of the present invention etches the sensitive material layer 301 from the back side (i.e., the first surface) of the sensitive material layer 301 to expose the interface layer 306, thereby making it possible to remove the interface layer 306.

[0079] Next, execute step S250, such as Figure 3DAs shown, a filling layer filling the groove 307 is formed. Exemplarily, a lift-off process may be used to form the filling layer filling the groove 307, that is, a photoresist layer is first formed outside the groove 307, and then a filling layer material is deposited to fill the groove 307 and cover the photoresist layer, and then the photoresist layer and the filling layer outside the groove 307 are removed together, and the filling layer filled inside the groove 307 is retained. Alternatively, a material with a relatively high etching selectivity with the sensitive material layer 301 may be selected to form the filling layer, and after the filling layer material is deposited, the filling layer material outside the groove 307 is removed by photolithography and etching, and the filling layer inside the groove 307 is retained.

[0080] In order to avoid re-forming an interface layer at the bottom of the groove 307 during the process of forming the filling layer, the filling layer material can be deposited under vacuum conditions to form the filling layer. Exemplarily, the vacuum condition means that the air pressure in the space where the deposition process is performed is less than one atmosphere. Depositing the filling layer material under vacuum conditions can prevent the sidewall layer 304 exposed at the bottom of the groove 307 and the sensitive material layer 301 exposed on the sidewall from being oxidized.

[0081] On the other hand, the filling layer material can be a material that is difficult to oxidize, that is, the filling layer material is at least more difficult to oxidize than the sensitive material layer 301; for example, the filling layer material can be platinum (Pt). Using a material that is difficult to oxidize to form the filling layer can avoid forming another form of interface layer at the bottom and sidewall of the groove 307 due to oxidation of the filling layer material itself.

[0082] Next, execute step S260, such as Figure 3E As shown, the sacrificial layer is removed through the release hole 305 to form a cavity structure between the sidewall layer 304 and the sensitive material layer 301 .

[0083] As described above, in order to expose the first surface of the sensitive material layer 301 to form the groove 307, a second substrate is first formed on the sidewall layer 304 as a temporary substrate. Therefore, in order to expose the release hole 305 to remove the sacrificial layer, a third substrate may be first formed on the first surface of the sensitive material layer, for example, by gluing or bonding; then the second substrate is removed to expose the release hole 305.

[0084] The release hole 305 is formed above the sacrificial layer 303, thereby exposing the top of the sacrificial layer 303. The etchant can remove the sacrificial layer 303 through the release hole 305, thereby forming a cavity structure surrounded by the sidewall layer 304 and the sensitive material layer 301. In the process of etching the sacrificial layer, the etchant will react with the interface layer 306, thereby causing a certain degree of lateral corrosion to the interface layer 306. However, since the embodiment of the present invention removes the middle part of the interface layer 306 through the groove 307, only a small amount of the interface layer is retained around the groove 307, thereby limiting the maximum distance of the interface layer 306 to be laterally corroded, and reducing the possibility of cracking between the sidewall layer 304 and the sensitive material layer 301.

[0085] At this point, the process steps implemented in the method for manufacturing a semiconductor device according to an embodiment of the present invention have been completed. It can be understood that the method for manufacturing a semiconductor device according to the embodiment of the present invention not only includes the above steps, but may also include other necessary steps before, during or after the above steps, which are all included in the scope of the manufacturing method according to the embodiment of the present invention.

[0086] According to the method for manufacturing a semiconductor device provided by the present invention, by forming a groove penetrating the sensitive material layer and removing the interface layer through the groove, cracking between the sidewall layer and the sensitive material layer caused by corrosion of the interface layer can be avoided, thereby enhancing the overall structure of the semiconductor device.

[0087] like Figure 3E As shown, an embodiment of the present invention further provides a semiconductor device, which can be manufactured by the manufacturing method of the semiconductor device as described above. Specifically, the semiconductor device of the embodiment of the present invention includes: a sensitive material layer 301, the sensitive material layer 301 includes a first surface and a second surface opposite to the first surface; a sidewall layer 304 formed on the second surface of the sensitive material layer 301; a groove 307 penetrating the sensitive material layer from the first surface of the sensitive material layer 301, the opening position of the groove 307 is arranged opposite to the bottom of the sidewall layer 304, the groove 307 is filled with a filling layer, and the bottom of the filling layer is connected to the bottom of the sidewall layer 304; a cavity structure arranged between the sidewall layer 304 and the sensitive material layer 301.

[0088] In some embodiments, the sensitive material layer 301 may be a piezoelectric layer; the semiconductor device further includes a first electrode (not shown) formed on a first surface of the sensitive material layer, and a second electrode 302 formed on a second surface of the sensitive material layer. The first electrode, the piezoelectric layer, and the second electrode constitute a composite film, which may also include other film layers in addition to the above-mentioned film layers, and may be reasonably arranged according to the actual device, and is not specifically limited here.

[0089] The semiconductor device of the embodiment of the present invention is formed with a groove penetrating the sensitive material layer. There is no interface layer at the bottom of the groove, which can avoid cracking between the sidewall layer and the sensitive material layer due to corrosion of the interface layer, thereby enhancing the overall structure of the semiconductor device.

[0090] The present invention has been described by the above embodiments, but it should be understood that the above embodiments are only for the purpose of example and description, and are not intended to limit the present invention to the scope of the described embodiments. In addition, it can be understood by those skilled in the art that the present invention is not limited to the above embodiments, and more variations and modifications can be made according to the teachings of the present invention, and these variations and modifications all fall within the scope of the protection claimed by the present invention. The protection scope of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for manufacturing a semiconductor device, characterized in that: The method comprises: Providing a sensitive material layer, the sensitive material layer comprising a first surface and a second surface opposite to the first surface; A sacrificial layer and a sidewall layer surrounding the sacrificial layer are formed on the second surface of the sensitive material layer, a release hole connected to the sacrificial layer is formed on the top of the sidewall layer, and an interface layer is formed between the bottom of the sidewall layer and the second surface of the sensitive material layer; Etching the sensitive material layer from the first surface of the sensitive material layer to form a groove penetrating the sensitive material layer, wherein the opening position of the groove is arranged opposite to the bottom of the sidewall layer, and the bottom of the groove exposes the interface layer; removing the interface layer exposed at the bottom of the groove; forming a filling layer filling the groove; The sacrificial layer is removed through the release hole to form a cavity structure between the sidewall layer and the sensitive material layer.

2. The manufacturing method according to claim 1, characterized in that The removing the interface layer exposed at the bottom of the groove comprises: The interface layer is physically bombarded to remove the interface layer.

3. The manufacturing method according to claim 1, characterized in that: The removing the interface layer exposed at the bottom of the groove comprises: The interface layer is reduced by using a reducing agent to remove the interface layer.

4. The manufacturing method according to claim 1, characterized in that: The forming of a filling layer filling the groove comprises: The filling layer material is deposited under vacuum conditions to form the filling layer.

5. The manufacturing method according to claim 4, characterized in that: The filling layer material is a material that is more difficult to oxidize than the sensitive material layer.

6. The manufacturing method according to claim 1, characterized in that: The width of the groove is smaller than the width of the bottom of the sidewall layer.

7. The manufacturing method according to claim 1, characterized in that: Providing the sensitive material layer comprises: providing a first substrate, and forming the sensitive material layer on the first substrate, wherein the first surface of the sensitive material layer is disposed on the first substrate; Before forming the groove, the method further includes: forming a second substrate on top of the sidewall layer; The first substrate is removed to expose the first surface of the sensitive material layer.

8. The manufacturing method according to claim 7, characterized in that: After forming the filling layer, the method further includes: forming a third substrate on the first surface of the sensitive material layer; The second substrate is removed to expose the release hole.

9. The manufacturing method according to any one of claims 1 to 8, characterized in that: The sensitive material layer includes a piezoelectric layer. A first electrode is formed on the first surface of the sensitive material layer. A second electrode is formed on the second surface of the sensitive material layer.

10. A semiconductor device, characterized in that: The semiconductor device comprises: a sensitive material layer, the sensitive material layer comprising a first surface and a second surface opposite to the first surface; a sidewall layer formed on the second surface of the sensitive material layer; A groove extending from the first surface of the sensitive material layer through the sensitive material layer, wherein the opening position of the groove is arranged opposite to the bottom of the sidewall layer, the groove is filled with a filling layer, and the bottom of the filling layer is connected to the bottom of the sidewall layer; A cavity structure is arranged between the sidewall layer and the sensitive material layer.