Method for recycling phosphorus resource in solid steel slag

By treating solid steel slag using a low-temperature solid-state reduction method, P2O5 is generated for use in phosphate chemical production, and the dephosphorized tailings are used in converter steelmaking. This solves the problem of low efficiency in solid steel slag treatment and achieves efficient recovery of phosphorus resources and efficient utilization of steel slag.

CN118929592APending Publication Date: 2024-11-12UNIV OF SCI & TECH BEIJING

Patent Information

Application Number
CN202410995501.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing technologies are insufficient for efficiently processing phosphorus resources in solid steel slag, resulting in low utilization efficiency. Furthermore, heating it to a molten state requires the consumption of large amounts of fuel and causes environmental pollution.

Method used

After crushing and grinding solid steel slag and metallurgical coke using a low-temperature solid-state reduction method, the mixture undergoes a low-temperature reduction dephosphorization reaction in a gas-fired furnace. The generated phosphorus element is recovered through steam to generate P2O5 for use in phosphorus chemical production. The tailings after dephosphorization can be directly used as a slagging agent in converter steelmaking.

Benefits of technology

This method enables the efficient recovery and utilization of phosphorus in solid steel slag, reduces processing costs, minimizes environmental pollution, improves the utilization efficiency of steel slag, and enhances the economic benefits of steel enterprises.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004960050360000041
    Figure BDA0004960050360000041
  • Figure BDA0004960050360000042
    Figure BDA0004960050360000042
  • Figure BDA0004960050360000051
    Figure BDA0004960050360000051
Patent Text Reader

Abstract

The invention belongs to the technical field of ferrous metallurgy, and particularly relates to a method for recycling phosphorus resources in solid-state steel slag, the solid-state steel slag is subjected to low-temperature solid-state reduction dephosphorization treatment, phosphorus in the slag is discharged in the form of P2, the high dephosphorization rate can be obtained, and phosphorus steam generates P2O5 through phosphorus recycling equipment to be used for phosphorus chemical industry production. The content of phosphorus in the dephosphorized slag is low, the dephosphorized solid steel slag can be directly reused in the converter steelmaking process, and finally the purpose of efficient utilization of the solid steel slag is achieved. The method is simple, reliable and high in dephosphorization efficiency, dephosphorized products can be used for manufacturing phosphate fertilizer and other high-added-value products, dephosphorized tailings are directly reused in the converter steelmaking process, consumption of slagging materials is reduced, the pretreatment time is shortened, meanwhile, heat loss in the converter steelmaking slagging process is reduced, industrial solid waste emission and environment pollution are reduced, and the method is suitable for industrial production. The economic benefits of iron and steel enterprises are increased, and the method has important reference and guiding significance on efficient recycling of metallurgical industrial waste residues.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a method for recovering phosphorus resources in solid steel slag. Background Art

[0002] Steel slag is the main by-product of the steelmaking process, which has an important impact on the quality of molten steel. It has the characteristics of large emissions, large pollution, and high processing costs. Waste steel slag not only occupies land resources, but the heavy metal elements in the slag are seriously harmful to the soil and human body. Steel slag contains valuable components such as iron, phosphorus, and manganese, which have great recycling value. At present, magnetic separation is widely used in the mainstream steel slag dephosphorization process. The equipment required for magnetic separation is simple, easy to operate, and low in cost, but the one-time treatment efficiency is low. Carbon thermal reduction dephosphorization is to use P2O5 to have better reduction properties than other oxides, and to add a carbonaceous reducing agent to react with P2O5 to generate P2 gasification and removal. The dephosphorization rate of the carbon thermal reduction method is 80-95%, which has the characteristics of low cost, simple equipment, environmental friendliness, and suitability for industrial production. The Chinese patent applications with publication numbers CN108998605A and CN116926247A use the carbon thermal reduction method to perform carbon thermal reduction dephosphorization on hot steel slag, and add a carbonaceous reducing agent to the hot steel slag to achieve the purpose of dephosphorization. At present, all the existing patents on carbon thermal reduction dephosphorization are for the treatment of hot molten steel slag, but the current untreated solid steel slag stock is huge and the treatment and utilization efficiency is low. Heating solid steel slag to a molten state consumes a lot of fuel and equipment costs, and the process also generates environmental pollution. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a method for recovering phosphorus resources in solid steel slag.

[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0005] A method for recovering phosphorus resources from solid steel slag comprises the following steps:

[0006] S1. The solid slag and metallurgical coke are crushed and ground respectively, and then mixed in proportion to obtain a mixture;

[0007] S2. The mixture is placed in a gas-fired heating furnace for solid-state low-temperature reduction dephosphorization reaction;

[0008] S3. The phosphorus element is collected in the vapor recovery tank to generate P2O5, which is used in the phosphorus chemical industry to produce phosphorus-containing products;

[0009] S4. The tailings after solid-state low-temperature reduction dephosphorization can be directly added to the converter steelmaking process as a slag-making agent.

[0010] As a preferred embodiment of the method for recovering phosphorus resources in solid steel slag described in the present invention, in step S1, a planetary ball mill is used to crush and grind the solid steel slag and metallurgical coke respectively, and the particle sizes of the solid steel slag and metallurgical coke after grinding are both 5 to 20 μm.

[0011] As a preferred embodiment of the method for recovering phosphorus resources from solid steel slag described in the present invention, in step S1, the mass ratio of solid steel slag to metallurgical coke is 1:(0.2-0.5).

[0012] As a preferred solution of the method for recovering phosphorus resources in solid steel slag described in the present invention, wherein: in step S2, the fuel gas is blast furnace gas.

[0013] As a preferred solution of the method for recovering phosphorus resources in solid steel slag described in the present invention, wherein: in the step S2, the reaction temperature is 900-1200°C, and the reaction time is 20-60 minutes.

[0014] As a preferred embodiment of the method for recovering phosphorus resources from solid steel slag according to the present invention, in step S4, the tailings after solid low-temperature reduction dephosphorization are directly added to the converter steelmaking process as a converter slag-making agent, and the addition amount is 5-8 kg / t 钢 .

[0015] The beneficial effects of the present invention are as follows:

[0016] The present invention proposes a method for realizing phosphorus resource recovery in solid steel slag, wherein the solid steel slag is subjected to low-temperature solid-state reduction dephosphorization treatment, and phosphorus in the slag is discharged in the form of P2, so that a higher dephosphorization rate can be obtained, and phosphorus vapor is converted into P2O5 for phosphorus chemical production through phosphorus recovery equipment. The phosphorus content in the slag after dephosphorization is low, and the solid steel slag after dephosphorization can be directly reused in the converter steelmaking process, and finally the purpose of efficient utilization of solid steel slag is achieved. The method is simple and reliable, with high dephosphorization efficiency, and the dephosphorization product can be used to manufacture high value-added products such as phosphate fertilizer, and the dephosphorization tailings are directly reused in the converter steelmaking process, which not only reduces the consumption of slag-making materials and shortens the pretreatment time, but also reduces the heat loss in the converter steelmaking slag-making process, reduces industrial solid waste emissions and environmental pollution, increases the economic benefits of steel enterprises, and also has important reference and guiding significance for the efficient recycling of metallurgical industrial waste slag. DETAILED DESCRIPTION

[0017] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] According to one aspect of the present invention, the present invention provides the following technical solution:

[0019] A method for recovering phosphorus resources from solid steel slag comprises the following steps:

[0020] S1. The solid slag and metallurgical coke are crushed and ground respectively, and then mixed in proportion to obtain a mixture;

[0021] S2. The mixture is placed in a gas-fired heating furnace for solid-state low-temperature reduction dephosphorization reaction;

[0022] S3. The phosphorus element is collected in the vapor recovery tank to generate P2O5, which is used in the phosphorus chemical industry to produce phosphorus-containing products;

[0023] S4. The tailings after solid-state low-temperature reduction dephosphorization can be directly added to the converter steelmaking process as a slag-making agent.

[0024] Preferably, in step S1, a planetary ball mill is used to crush and grind the solid steel slag and metallurgical coke respectively, and the particle size of the solid steel slag and metallurgical coke after grinding is 5 to 20 μm, and the mass ratio of solid steel slag to metallurgical coke is 1: (0.2 to 0.5). Specifically, the particle size of the solid steel slag and metallurgical coke after grinding can be, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, any one of them or any two of them, and the mass ratio of solid steel slag to metallurgical coke can be, for example, 1: 0.2, 1: 0.3, 1: 0.4, 1: 0.5, any one of them or any two of them.

[0025] Preferably, in step S2, the reaction temperature is 900-1200°C, the fuel gas is blast furnace gas, the reaction time is 20-60 min, and phosphorus in the slag reacts to generate P2 vapor. Specifically, the reaction temperature can be, for example, any one of 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1500°C, 2000°C, or a range between any two thereof, and the reaction time can be, for example, any one of 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, or a range between any two thereof.

[0026] Preferably, in step S4, the tailings after solid-state low-temperature reduction dephosphorization are directly added to the converter steelmaking process as a converter slag-making agent, and the addition amount is 5-8 kg / t 钢 Specifically, the amount added can be, for example, 5 kg / t 钢 、5.5kg / t 钢 、6kg / t 钢 、6.5kg / t钢 , 7kg / t 钢 、7.5kg / t 钢 , 8kg / t 钢 Any one of them or the range between any two of them.

[0027] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0028] Example 1

[0029] This method is used to dephosphorize the solid steel slag piled up in the converter steelmaking process of a certain factory. The specific implementation process is as follows: Grind the solid steel slag and metallurgical coke to 6μm, the mass ratio of solid steel slag to metallurgical coke is 1:0.5, and add them into the gas heating furnace after sufficient mixing. The fuel gas is blast furnace gas. The reaction temperature is controlled at 1150℃ and the reaction time is 50min. The dephosphorized solid steel slag can be reused in the converter steelmaking process in a hot state as a slag-making agent, and the addition amount is 6kg / t 钢 .

[0030] The composition of the solid slag before and after low-temperature solid-state reduction of the solid slag from converter steelmaking in this embodiment is shown in Table 1. As can be seen from Table 1, after being treated by the method of the present invention, the P2O5 content in the solid slag is reduced from 3.52wt% to 0.67wt%, and the dephosphorization effect is significant. The solid slag can be directly added to the converter steelmaking process as a slag-making agent to achieve efficient utilization of the solid slag from converter steelmaking.

[0031] Table 1 Solid slag composition before and after dephosphorization (wt%)

[0032]

[0033] Example 2

[0034] This method is used to dephosphorize the solid steel slag piled up in the converter steelmaking process of a certain factory. The specific implementation process is as follows: Grind the solid steel slag and metallurgical coke to 13μm, the mass ratio of solid steel slag to metallurgical coke is 1:0.4, and add them to the gas heating furnace after sufficient mixing. The fuel gas is blast furnace gas. The reaction temperature is controlled at 1050℃ and the reaction time is 30min. The dephosphorized solid steel slag can be reused in the converter steelmaking process in a hot state as a slag-making agent, and the addition amount is 5kg / t 钢 .

[0035] The composition of the solid slag before and after low-temperature solid-state reduction of the converter steelmaking solid slag with metallurgical coke in this embodiment is shown in Table 2. As can be seen from Table 2, after being treated by the method of the present invention, the P2O5 content in the solid slag is reduced from 3.52wt% to 0.93wt%, and the dephosphorization effect is significant. The solid slag can be directly added to the converter steelmaking process as a slag-making agent to achieve efficient utilization of the solid slag from converter steelmaking.

[0036] Table 2 Solid slag composition before and after dephosphorization (wt%)

[0037]

[0038] Comparative Example 1

[0039] The difference compared with Example 1 is that the mass ratio of solid steel slag to metallurgical coke is 1:0.1.

[0040] The composition of the solid slag before and after low-temperature solid-state reduction of the solid slag from converter steelmaking in this comparative example is shown in Table 3. As can be seen from Table 3, after being treated by the method of the present invention, the P2O5 content in the solid slag is reduced from 3.52wt% to 1.78wt%, and the dephosphorization effect is not good. The tailings cannot be added to the converter steelmaking process as a slag-making agent.

[0041] Table 4 Solid slag composition before and after dephosphorization (wt%)

[0042]

[0043]

[0044] Comparative Example 2

[0045] The difference compared with Example 1 is that the reaction temperature is 800°C.

[0046] The composition of the solid slag before and after low-temperature solid-state reduction of the solid slag from converter steelmaking in this comparative example is shown in Table 4. As can be seen from Table 4, after being treated by the method of the present invention, the P2O5 content in the solid slag is reduced from 3.52wt% to 2.06wt%, and the dephosphorization effect is not good. The tailings cannot be added to the converter steelmaking process as a slag-making agent.

[0047] Table 5 Solid slag composition before and after dephosphorization (wt%)

[0048]

[0049] The present invention performs low-temperature solid-state reduction dephosphorization treatment on solid steel slag, and phosphorus in the slag is discharged in the form of P2, so that a higher dephosphorization rate can be obtained, and phosphorus vapor is converted into P2O5 for phosphorus chemical production through phosphorus recovery equipment. The phosphorus content in the slag after dephosphorization is low, and the solid steel slag after dephosphorization can be directly reused in the converter steelmaking process, and finally the purpose of efficient utilization of solid steel slag is achieved. The method is simple and reliable, with high dephosphorization efficiency. The dephosphorization product can be used to manufacture high value-added products such as phosphate fertilizer, and the dephosphorization tailings are directly reused in the converter steelmaking process, which not only reduces the consumption of slag-making materials and shortens the pretreatment time, but also reduces the heat loss in the converter steelmaking slag-making process, reduces industrial solid waste emissions and environmental pollution, increases the economic benefits of steel enterprises, and also has important reference and guiding significance for the efficient recycling of metallurgical industrial waste slag.

[0050] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for recovering phosphorus resources from solid steel slag, characterized in that: The following steps are involved: S1. The solid slag and metallurgical coke are crushed and ground respectively, and then mixed in proportion to obtain a mixture; S2. The mixture is placed in a gas-fired heating furnace for solid-state low-temperature reduction dephosphorization reaction; S3. The phosphorus element is collected in the vapor recovery tank to generate P2O5, which is used in the phosphorus chemical industry to produce phosphorus-containing products; S4. The tailings after solid-state low-temperature reduction dephosphorization can be directly added to the converter steelmaking process as a slag-making agent.

2. The method for recovering phosphorus resources from solid steel slag according to claim 1, characterized in that: In the step S1, a planetary ball mill is used to crush and grind the solid steel slag and the metallurgical coke respectively, and the particle sizes of the solid steel slag and the metallurgical coke after grinding are both 5-20 μm.

3. The method for recovering phosphorus resources from solid steel slag according to claim 1, characterized in that: In the step S1, the mass ratio of solid steel slag to metallurgical coke is 1:(0.2-0.5).

4. The method for recovering phosphorus resources from solid steel slag according to claim 1, characterized in that: In step S2, the fuel gas is blast furnace gas.

5. The method for recovering phosphorus resources from solid steel slag according to claim 1, characterized in that: In step S2, the reaction temperature is 900-1200° C., and the reaction time is 20-60 min.

6. The method for recovering phosphorus resources from solid steel slag according to claim 1, characterized in that: In step S4, the tailings after solid-state low-temperature reduction dephosphorization are directly added to the converter steelmaking process as a converter slag-making agent, and the addition amount is 5-8 kg / t 钢 .

Citation Information

Patent Citations

  • Full-amount utilization method of steel slag

    CN112624070A

  • Steel slag total utilization technology based on low-carbon dephosphorization of molten slag

    CN116855647A

  • Converter steel slag thermal-state cycle full-amount utilization method

    CN118166172A

  • Method for recovering iron and phosphorus from steelmaking slag

    JP2012219298A

Cited By

  • Rare earth electroslag steel containing alloyed rare earth elements and manufacturing method of rare earth electroslag steel

    CN121428279A