Potassium ion doped sodium vanadium phosphate positive electrode material and preparation method and application thereof

Through the preparation method of potassium ion doped sodium vanadium phosphate positive electrode material, the problems of structural damage and insufficient conductivity of Na3V2(PO4)3 positive electrode material during sodium ion removal and embedding are solved, and the cycle stability and rate performance are improved, so as to achieve Improved high discharge specific capacity and electrochemical performance.

CN118929609APending Publication Date: 2024-11-12CHINA UNIV OF GEOSCIENCES (WUHAN)
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411032149.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing Na3V2 (PO4)3 positive electrode material has irreversible structural damage and phase change during sodium ions detachment and embedding, resulting in poor cyclic stability and rate performance. The inappropriate preparation method leads to sodium ions diffusion obstacles and electronic conductivity. The discharge specific capacity and stability of the electrode are reduced.

Method used

The preparation method of potassium ion doped vanadium phosphate positive electrode material is adopted. By mixing salts containing sodium, phosphorus, vanadium and potassium with sucrose and anhydrous oxalic acid, spray-drying, sintering in a tube furnace to form Na3-xV2Kx ( PO4)3/C composite electrode material increases the structural support of potassium ions, forms a carbon cladding layer, and improves ionic and electron conductivity.

Benefits of technology

The cyclic stability and rate performance of the electrode material are significantly improved, the discharge specific capacity is increased, the diffusion rate and electron conductivity of sodium ions are improved, and the electrode material with high energy density and long life is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929609A_ABST
    Figure CN118929609A_ABST
Patent Text Reader

Abstract

The invention discloses a potassium ion doped sodium vanadium phosphate positive electrode material and a preparation method and application thereof. The invention relates to the technical field of electrode materials. The preparation method comprises the following steps: S1, mixing salt containing sodium element, phosphorus element, vanadium element and potassium element with cane sugar, deionized water and anhydrous oxalic acid, putting the mixture into a beaker, and fully mixing and dissolving to form a uniform mixed solution; s2, performing spray drying on the mixed solution in the S1 to obtain powder; and S3, sintering the powder prepared in the step S2 in a tubular furnace to obtain the potassium ion doped sodium vanadium phosphate positive electrode material. The potassium ion doped sodium vanadium phosphate positive electrode material prepared by the invention has relatively high specific discharge capacity and coulombic efficiency and excellent cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrode materials, and in particular to a potassium ion-doped sodium vanadium phosphate positive electrode material and a preparation method and application thereof. Background Art

[0002] Metallic sodium is an environmentally friendly battery material because it is more abundant in resources and safer than metallic lithium. Therefore, the development and application of sodium-ion batteries are very green, environmentally friendly and cost-effective, and have great commercial value and research and development enthusiasm. The main goal of the research and development of sodium-ion battery electrode materials, especially sodium-ion battery positive electrode materials with great energy storage advantages, is to improve energy conversion efficiency and reduce energy consumption. With the large-scale promotion of electric vehicles and electric vehicles and the continuous consumption of non-renewable energy, the demand for energy storage in today's society is increasing day by day, and green and environmentally friendly energy technologies are urgently needed.

[0003] Na3V2(PO4)3 is a typical NASICON-type cathode material with a large three-dimensional open channel structure, which facilitates the rapid extraction and insertion of sodium ions. When the Na3V2(PO4)3 electrode is charged and discharged, a reversible phase change reaction occurs, and the crystal structure changes to Na3V2(PO4)3-NaV2(PO4)3-Na3V2(PO4)3. This process corresponds to V 4+ / V 3+ The redox process, V 4+ / V 3 + The redox voltage is 3.3V / 3.4V, so the charge and discharge platform of Na3V2(PO4)3 electrode is 3.3V / 3.4V. Although vanadium-based polyanionic compounds have potential advantages such as higher voltage platform, higher energy density and good stability. However, during the extraction and embedding of sodium ions, irreversible structural damage and inevitable phase changes and side reactions will occur, resulting in poor cycle stability and poor rate performance; at the same time, if the preparation method is not suitable, it will bring about greater sodium ion diffusion obstacles and poor electronic conductivity, which will significantly reduce the discharge specific capacity and cycle stability of the Na3V2(PO4)3 electrode.

[0004] The methods to overcome the disadvantages of Na3V2(PO4)3 materials such as unstable structure and weak conductivity during charge and discharge include microscopic unit cell structure regulation, structural nano-sizing, carbon-based material composite and a combination of these. Metal ion doping is a method of unit cell structure regulation, which can effectively achieve higher energy density and cycle stability, and is conducive to large-scale energy conversion and storage. Therefore, the development and application of higher performance Na3V2(PO4)3 electrode materials is very necessary. Summary of the invention

[0005] The purpose of the present invention is to address the above-mentioned deficiencies in the prior art and to provide a potassium ion-doped sodium vanadium phosphate positive electrode material having higher discharge specific capacity and coulombic efficiency and excellent cycle stability, as well as a preparation method and application thereof.

[0006] A method for preparing a potassium ion-doped sodium vanadium phosphate positive electrode material of the present invention comprises the following steps:

[0007] S1. Mix salt containing sodium, phosphorus, vanadium and potassium with sucrose, deionized water and anhydrous oxalic acid in a beaker, mix and dissolve them thoroughly to form a uniform mixed solution;

[0008] S2, spray drying the mixed solution of S1 to obtain powder;

[0009] S3. Sintering the powder obtained in step S2 in a tube furnace to obtain a potassium ion-doped sodium vanadium phosphate positive electrode material.

[0010] Furthermore, in step S1, in the salt containing sodium, phosphorus, vanadium and potassium, the molar ratio of sodium, potassium, phosphorus and vanadium is 2.8-2.99:0.01-0.2:3:2, the molar ratio of oxalic acid to vanadium is 4:1, and the mass of sucrose is 5% to 20% of the sum of the mass of the salt, sucrose and anhydrous oxalic acid.

[0011] Furthermore, in step S1, the sodium source is sodium dihydrogen phosphate, the phosphorus source is sodium dihydrogen phosphate and potassium dihydrogen phosphate, the vanadium source is vanadium pentoxide or ammonium metavanadate, the potassium source is potassium dihydrogen phosphate or potassium carbonate, and the carbon source is oxalic acid or citric acid.

[0012] Furthermore, in step S2, the spray drying condition is an inlet temperature of 150°C-200°C.

[0013] Furthermore, in step S2, the spray drying condition is a feed rate of 10-20 ml / min.

[0014] Furthermore, in step S3, the atmosphere of the tube furnace is nitrogen.

[0015] Furthermore, in step S3, the powder calcination temperature is 750-800° C., the heating rate is 1-7° C. / min, and the calcination time is 8-10 h.

[0016] A potassium ion-doped sodium vanadium phosphate positive electrode material prepared by the above-mentioned preparation method, wherein the chemical formula of the positive electrode material is Na 3-x V2K x (PO4)3 / C, X is 0.01-0.2.

[0017] Furthermore, Na 3-x V2K xThe (PO4)3 / C composite electrode material is hollow spherical, and a carbon coating layer of uniform thickness is formed on its surface.

[0018] An application of the potassium ion-doped sodium vanadium phosphate positive electrode material in a sodium battery.

[0019] The potassium ions described in the present invention replace Na in an appropriate amount, which will play a structural supporting role, causing the unit cell volume to increase, the C axis to lengthen, and the Na + The transmission channel is beneficial to improving the ionic conductivity of the electrode material, thereby improving the cycle stability and rate performance of the material.

[0020] In the present invention, a carbon source is added to the mixed solution to be in situ coated on Na3V during the spray drying process. 2-x M x The surface of (PO4)3 / C precursor particles can prevent Na3V 2-x M x The (PO4)3 / C precursor particles grow and agglomerate; they can also be thermally decomposed into amorphous carbon during heat treatment to form small spherical Na3V 2-x M x (PO4)3 / C particles. The particles have a nano-microsphere structure with rich pores inside. On the one hand, it can increase the contact area between the active material and the electrolyte, shorten the sodium ion transmission path, and increase the sodium ion diffusion rate. On the other hand, it can improve the electronic conductivity by simply coating the carbon material in situ, which is very important for improving the Na3V 2-x M x It has a huge promoting effect on the electrochemical performance of (PO4)3 / C electrode materials.

[0021] The method of the invention is simple, has low cost and can be produced on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 XRD diagrams of the sodium vanadium phosphate positive electrode material prepared in Comparative Example 1 and the potassium ion-doped sodium vanadium phosphate positive electrode material prepared in Example 2 of the present invention;

[0023] Figure 2 This is a FESEM image of the potassium ion-doped sodium vanadium phosphate positive electrode material prepared in Example 2 of the present invention;

[0024] Figure 3 This is a TEM image of the potassium ion-doped sodium vanadium phosphate positive electrode material prepared in Example 2 of the present invention;

[0025] Figure 4 This is a nitrogen adsorption-desorption curve of the potassium ion-doped sodium vanadium phosphate positive electrode material prepared in Example 2;

[0026] Figure 5The sodium vanadium phosphate positive electrode material prepared in Comparative Example 1 and the Na prepared in Example 2 of the present invention 3-x V2K x (PO4)3 / C material has a voltage range of 2.5-3.8V and a 1C (1C = 117 mAh g -1 ) Typical discharge capacity curve under current density;

[0027] Figure 6 The sodium vanadium phosphate positive electrode material prepared in Comparative Example 1 and the Na prepared in Examples 1-3 of the present invention 3-x V2K x Typical discharge capacity curves of (PO4)3 / C materials in the voltage range of 2.5-3.8V and at different current densities of 0.2C-10C;

[0028] Figure 7 The sodium vanadium phosphate positive electrode material prepared in Comparative Example 1 and the Na prepared in Example 2 of the present invention 3-x V2K x Electrochemical impedance spectroscopy of (PO4)3 / C electrode in the range of 100000-0.01 Hz. DETAILED DESCRIPTION

[0029] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0030] Example 1

[0031] This embodiment involves a method for preparing a metal-doped sodium vanadium phosphate composite electrode material, and the preparation method is as follows:

[0032] S1. Weigh 3.599 g (0.03 mol) of sodium dihydrogen phosphate (relative molecular mass 119.98), 1.819 g (0.01 mol) of vanadium pentoxide (relative molecular mass 181.88), 3.6012 g (0.04 mol) of oxalic acid (relative molecular mass 90.03), 0.068 g (0.0005 mol) of potassium dihydrogen phosphate (relative molecular mass 136.09), and 10% of the total weight of sucrose into a beaker, add 50 mL of deionized water, stir with a glass rod, and mix thoroughly.

[0033] S2. The uniformly mixed solution is spray dried. The equipment setting parameters are as follows: inlet temperature 190°C, feed rate 10ml / min, spray atmosphere air, and powder is obtained by spray drying.

[0034] S3. Sintering the powder obtained in step S2 in a tubular furnace, wherein the atmosphere of the tubular furnace is nitrogen, the powder calcination temperature is 800° C., the heating rate is 3° C. / min, and the calcination time is 10 h to obtain a potassium ion-doped sodium vanadium phosphate positive electrode material.

[0035] Example 2

[0036] S1. Weigh 3.599 g (0.03 mol) of sodium dihydrogen phosphate (relative molecular mass 119.98), 1.819 g (0.01 mol) of vanadium pentoxide (relative molecular mass 181.88), 3.6012 g (0.04 mol) of oxalic acid (relative molecular mass 90.03), 0.136 g (0.001 mol) of potassium dihydrogen phosphate (relative molecular mass 136.09), and sucrose (mass fraction of 10% of the total weight of the substance) into a beaker, add 50 mL of deionized water, stir with a glass rod, and mix thoroughly.

[0037] S2. The uniformly mixed solution is spray dried. The equipment setting parameters are as follows: inlet temperature of 190°C, feed rate of 10 mL / min, spray atmosphere of air, and powder is obtained by spray drying.

[0038] S3. Sintering the powder obtained in step S2 in a tubular furnace, wherein the atmosphere of the tubular furnace is nitrogen, the powder calcination temperature is 800° C., the heating rate is 3° C. / min, and the calcination time is 10 h to obtain a potassium ion-doped sodium vanadium phosphate positive electrode material.

[0039] Example 3

[0040] S1. Weigh 3.599 g (0.03 mol) of sodium dihydrogen phosphate (relative molecular mass 119.98), 1.819 g (0.01 mol) of vanadium pentoxide (relative molecular mass 181.88), 3.6012 g (0.04 mol) of oxalic acid (relative molecular mass 90.03), 0.204 g (0.0015 mol) of potassium dihydrogen phosphate (relative molecular mass 136.09), and 10% of the total weight of sucrose into a beaker, add 50 mL of deionized water, stir with a glass rod, and mix thoroughly.

[0041] S2. The uniformly mixed solution is spray dried. The equipment setting parameters are as follows: inlet temperature 190°C, feed rate 10mLUY / min, spray atmosphere is air, and powder is obtained by spray drying.

[0042] S3. Sintering the powder obtained in step S2 in a tubular furnace, wherein the atmosphere of the tubular furnace is nitrogen, the powder calcination temperature is 800° C., the heating rate is 5° C. / min, and the calcination time is 10 h to obtain a potassium ion-doped sodium vanadium phosphate positive electrode material.

[0043] Comparative Example 1

[0044] S1. Weigh 3.599 g (0.03 mol) of sodium dihydrogen phosphate (relative molecular mass 119.98), 1.819 g (0.01 mol) of vanadium pentoxide (relative molecular mass 181.88), 3.6012 g (0.04 mol) of oxalic acid (relative molecular mass 90.03), and 10% of the total weight of sucrose into a beaker, add 50 mL of deionized water, stir with a glass rod, and mix thoroughly.

[0045] S2. The uniformly mixed solution is spray dried. The equipment setting parameters are as follows: inlet temperature 190°C, feed rate 10ml / min, spray atmosphere air, and powder is obtained by spray drying.

[0046] S3. Sintering the powder obtained in step S2 in a tubular furnace, wherein the atmosphere of the tubular furnace is nitrogen, the powder calcination temperature is 800° C., the heating rate is 3° C. / min, and the calcination time is 10 h to obtain a potassium ion-doped sodium vanadium phosphate positive electrode material.

[0047] The difference between Comparative Example 1 and Example 2 is that potassium dihydrogen phosphate is not added during the synthesis stage.

[0048] The potassium ion-doped sodium vanadium phosphate cathode material prepared in Example 2 was assembled into a half-cell, the active cathode material, acetylene black and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 7:2:1, and then the mixture was dispersed in N-methyl-2-pyrrolidone (NMP) for 12 hours using a magnetic stirrer to form a uniform slurry, after which the slurry was coated on aluminum foil and finally dried in a vacuum oven at 120°C for 12 hours to remove NMP. The electrode sheet was prepared by cutting the aluminum foil into discs with a diameter of 10 mm, and the mass loading of the cut electrode sheet was 2 to 3 mg cm -2 CR2032 button cells were assembled in an argon glove box. Sodium metal sheets and glass fiber separators (GF / A) were used as counter electrodes and separators, respectively. The electrolyte was 1 mol L dissolved in ethylene carbonate / diethyl carbonate (EC / DEC) (volume ratio = 1:1) with 5% fluoroethylene carbonate (FEC). -1 NaClO4.

[0049] The metal-doped sodium vanadium phosphate composite electrode material obtained by the above-mentioned preparation method of the metal-doped sodium vanadium phosphate composite electrode material is Na 3-x V2K x (PO4)3 / C (x=0, 0.05, 0.1, 0.15) composite electrode materials.

[0050] Figure 1The XRD patterns of the sodium vanadium phosphate positive electrode material prepared in comparative example 1 and the potassium ion-doped sodium vanadium phosphate positive electrode material prepared in example 2 of the present invention are compared with the standard card, and the correspondence with the standard card is good, which proves that the prepared product is Na 3-x V2K x (PO4)3 / C.

[0051] Figure 2 This is a FESEM image of the potassium ion-doped sodium vanadium phosphate positive electrode material prepared in Example 2 of the present invention; it can be seen that Na 3-x V2K x The (PO4)3 / C material is in the form of microspheres with a diameter of 10-15μm.

[0052] Figure 3 This is a TEM image of the potassium ion-doped sodium vanadium phosphate positive electrode material prepared in Example 2; it can be seen that Na 3-x V2K x The (PO4)3 / C material is in the form of microspheres and is filled with pores.

[0053] Figure 4 This is a nitrogen adsorption / desorption curve of the potassium ion-doped sodium vanadium phosphate positive electrode material prepared in Example 2; it can be seen that Na 3-x V2K x (PO4)3 / C material has a large specific surface area and abundant internal pores.

[0054] Figure 5 The sodium vanadium phosphate positive electrode material prepared in Comparative Example 1 and the Na prepared in Example 2 of the present invention 3-x V2K x (PO4)3 / C material has a voltage range of 2.5-3.8V and a 1C (1C = 117 mAh g -1 ) The typical discharge capacity curve under current density. It can be seen from the figure that Na 3-x V2K x The discharge capacity of the (PO4)3 / C (X=0.1) cathode material is 108 mAh g -1 , the capacity retention rate is 98% after 600 cycles.

[0055] Figure 6 The sodium vanadium phosphate positive electrode material prepared in Comparative Example 1 and the Na prepared in Examples 1-3 of the present invention 3-x V2K x Typical discharge capacity curve of (PO4)3 / C material in the voltage range of 2.5-3.8V and at different current densities of 0.2C-10C. 3-x V2K x The discharge capacity of (PO4)3 / C (X = 0.05) cathode material at 0.2C current density is 107 mAh g-1 The discharge capacity at 10C current density is 89 mAh g -1 .

[0056] Na 3-x V2K x The discharge capacity of (PO4)3 / C (X = 0.1) cathode material at 0.2C current density is 110 mAh g -1 The discharge capacity at 10C current density is 95 mAh g -1 .

[0057] Na 3-x V2K x The discharge capacity of (PO4)3 / C (X = 0.15) cathode material at 0.2C current density is 98 mAh g -1 The discharge capacity at 10C current density is 90 mAh g -1 .

[0058] Figure 7 The sodium vanadium phosphate positive electrode material prepared in Comparative Example 1 and the Na prepared in Example 2 of the present invention 3-x V2K x Electrochemical impedance spectrum of (PO4)3 / C electrode in the range of 100000-0.01Hz. It can be seen from the figure that Na 3-x V2K x (PO4)3 / C(X=0.1) has a smaller electrochemical impedance, which proves that the doping of potassium ions effectively improves the conductivity of sodium vanadium phosphate.

[0059] For matters not mentioned above, the prior art applies.

[0060] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a potassium ion-doped sodium vanadium phosphate positive electrode material, Features: The steps include: S1. Mix salt containing sodium, phosphorus, vanadium and potassium with sucrose, deionized water and anhydrous oxalic acid in a beaker, mix and dissolve them thoroughly to form a uniform mixed solution; S2, spray drying the mixed solution of S1 to obtain powder; S3. Sintering the powder obtained in step S2 in a tube furnace to obtain a potassium ion-doped sodium vanadium phosphate positive electrode material.

2. The method for preparing the potassium ion-doped sodium vanadium phosphate positive electrode material according to claim 1, Features: In step S1, in the salt containing sodium, phosphorus, vanadium and potassium, the molar ratio of sodium, potassium, phosphorus and vanadium is 2.8-2.99:0.01-0.2:3:2, the molar ratio of oxalic acid to vanadium is 4:1, and the mass of sucrose is 5% to 20% of the sum of the mass of the salt, sucrose and anhydrous oxalic acid.

3. The method for preparing the potassium ion-doped sodium vanadium phosphate positive electrode material according to claim 1, Features: In step S1, the sodium source is sodium dihydrogen phosphate, the phosphorus source is sodium dihydrogen phosphate and potassium dihydrogen phosphate, the vanadium source is vanadium pentoxide or ammonium metavanadate, the potassium source is potassium dihydrogen phosphate or potassium carbonate, and the carbon source is oxalic acid or citric acid.

4. The method for preparing the potassium ion-doped sodium vanadium phosphate positive electrode material according to claim 1, Features: In step S2, the spray drying condition is an inlet temperature of 150°C-200°C.

5. The method for preparing the potassium ion-doped sodium vanadium phosphate positive electrode material according to claim 1, Features: In the step S2, the spray drying condition is a feed rate of 10-20 ml / min.

6. The method for preparing the potassium ion-doped sodium vanadium phosphate positive electrode material according to claim 1, Features: In the step S3, the atmosphere of the tube furnace is nitrogen.

7. The method for preparing the potassium ion-doped sodium vanadium phosphate positive electrode material according to claim 1, Features: In the step S3, the powder calcination temperature is 750-800° C., the heating rate is 1-7° C. / min, and the calcination time is 8-10 h.

8. A potassium ion-doped sodium vanadium phosphate positive electrode material prepared by the preparation method according to any one of claims 1 to 7, Features: The chemical formula of the positive electrode material is Na 3-x V 2 K x (PO 4 ) 3 / C, X is 0.01-0.

2.

9. The potassium ion-doped sodium vanadium phosphate positive electrode material according to claim 8, Features: Na 3-x V 2 K x (PO 4 ) 3 The / C composite electrode material is hollow spherical, and a carbon coating layer of uniform thickness is formed on its surface.

10. Use of the potassium ion-doped sodium vanadium phosphate positive electrode material as claimed in claim 8 in a sodium battery.

Citation Information

Patent Citations

  • Carbon-coated metal ion-doped sodium vanadium phosphate composite cathode material prepared by freeze drying method, as well as preparation method and application thereof

    CN106058202A

  • Doping modified sodium vanadium fluorophosphates positive electrode material and preparation method thereof

    CN108899505A

  • Sodium vanadium phosphate composite cathode material and preparation method thereof

    CN111994890A

  • Graphene composite potassium-silicon co-doped sodium vanadium phosphate composite material and preparation and application thereof

    CN114944479A

  • Method for preparing polyanionic positive electrode material for sodium-ion batteries

    WO2023071351A1