Synthesis method and application of sodium vanadium pyrophosphate / carbon composite material
By using sodium salt, vanadium-containing compounds, ammonium phosphate and citric acid in the positive electrode material of sodium ion battery, the NaVP2O7/rGO composite material is solved, the low conductivity and fast cycle attenuation of sodium pyrophosphate under high temperature and high pressure conditions are solved. , achieving the improvement of high cycle stability and conductivity, and is suitable for high temperature and high pressure applications of sodium ion batteries.
Patent Information
- Application Number
- CN202411418577.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-10-12
AI Technical Summary
The sodium vanadium pyrophosphate material has low conductivity and fast cycle attenuation under high temperature and high pressure conditions, which affects its application performance in sodium ion batteries.
Sol is heated and stirred in deionized water by sodium salt, vanadium-containing compounds, ammonium phosphate and citric acid, and NaVP2O7 precursor material is obtained after drying and ball milling, and then ultrasonic dispersion and hydrothermal reaction with graphene oxide to form NaVP2O7/ The rGO composite material is calcined in an inert atmosphere to form a sodium vanadium pyrophosphate/carbon composite material.
The conductivity and cyclic stability of the material are significantly improved, and the cycle attenuation rate is reduced to 0.01%, which improves the electrochemical performance and high temperature resistance of the positive electrode material of sodium ion battery.
Smart Images

Figure CN118929617A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sodium ion battery electrode materials, and in particular to a synthesis method of a sodium vanadium pyrophosphate / carbon composite material and application thereof. Background Art
[0002] People's demand for energy is increasing day by day, but currently it is mainly based on thermal power generation. However, the greenhouse effect of the homeland on which human beings depend is becoming increasingly serious, which has aroused people's attention to the issue of carbon emissions. Green renewable energy is an ideal energy source. Its intermittent characteristics require the configuration of energy storage equipment. Electrochemical energy storage equipment has attracted widespread attention due to its advantages such as high power conversion rate and controllable scale.
[0003] Sodium-ion batteries have abundant sodium reserves and excellent high and low temperature performance, which has triggered in-depth research by researchers. Polyanion materials are one of the main technical routes for positive electrode materials of sodium-ion batteries. According to the type of anions, they are classified into: phosphates, pyrophosphates, fluorophosphates, sulfates, silicates and many other types of materials. This type of material has a three-dimensional framework structure composed of strong covalent bonds and has high structural stability. Vanadium-based polyanion materials have abundant (V 2 + 、V 3+ 、V 4+ 、V 5+ ) valence state, the redox potential is relatively high. Among them, pyrophosphate NaVP 2 O 7 There is an obvious redox potential at 3.9V, and the theoretical specific capacity is about 108.1mAhg -1 , with a high theoretical energy density of 421Whkg -1 In addition, NaVP pyrophosphate 2 O 7 It has good stability under high temperature and high pressure conditions and has good application prospects in special application fields. However, the large framework structure of the pyrophosphate group ensures the thermal stability of the material, but also causes problems such as low conductivity and fast cycle decay. Researchers continue to improve it to optimize the electrochemical performance of the material. Summary of the invention
[0004] The method of the present invention aims to provide a synthesis method of a sodium vanadium pyrophosphate / carbon composite material and its application. The prepared sodium vanadium pyrophosphate / carbon composite material has a low cycle attenuation rate and good cycle stability, and is suitable for a positive electrode material of a sodium ion battery.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions: In one aspect, the present invention provides a method for synthesizing a sodium vanadium pyrophosphate / carbon composite material, comprising the following steps: (1) Sodium salt, vanadium-containing compound, ammonium phosphate, and citric acid are added to deionized water, heated and stirred to form a sol, the sol is dried to obtain a dry gel, and the dry gel is ball-milled to obtain NaVP 2 O 7 Precursor materials; (2) NaVP 2 O 7 Precursor materials and GO are added to deionized water and ultrasonically dispersed to form a mixed solution; the mixed solution is subjected to a hydrothermal reaction to obtain NaVP 2 O 7 Precursor / rGO suspension, in which GO is graphene oxide; (3) NaVP 2 O 7 The precursor / rGO suspension was filtered, washed, and dried to obtain a powder precipitate, which was then calcined in an inert atmosphere to obtain a sodium vanadium pyrophosphate / carbon composite material (NaVP 2 O 7 / rGO).
[0006] Furthermore, in the step (1), the molar ratio of the sodium salt, the vanadium-containing compound, the ammonium phosphate salt, and the citric acid is 10-13 mol:10 mol:20 mol:3 mol; the sodium salt is Na 2 CO 3 , NaCl, Na 2 C 2 O 4 One of the following; the vanadium-containing compound is NH 4 VO 3 or V 2 O 5 ; Ammonium phosphate is NH 4 H 2 PO 4 or (NH 4 ) 2 HPO 4 ; The ball-to-material ratio is 1:10~20, the rotation speed is 500~700r / min, and the grinding time is 3~8h.
[0007] Furthermore, in step (2), NaVP 2 O 7 The mass ratio of precursor material and GO is 10~30:1; the hydrothermal reaction temperature is 150~170℃; and the heating time is 5~10h.
[0008] Furthermore, in the step (3), the calcination temperature is 600°C to 800°C, and the calcination time is 8 to 10 hours.
[0009] On the other hand, the present invention also provides a method for using the sodium vanadium pyrophosphate / carbon composite material prepared by the above method as a positive electrode material for a sodium ion battery.
[0010] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: The pyrophosphate prepared by the traditional preparation method has poor conductivity, and the resistance of electrons and ions during the shuttling process is relatively large; the technical scheme of the present invention first adds sodium salt, vanadium-containing compound, ammonium phosphate and citric acid into deionized water, heats and stirs to carry out liquid phase reaction, so that the three carboxylic acid groups on the citric acid molecules are combined with vanadium metal ions to different degrees to form coordination polymers to form molecular chains, and the molecular chains are cross-linked with each other to gradually form a sol with a network framework structure; then the solvent molecules sealed in the network framework are evaporated through drying to form a network-like dry gel; the dry gel is ball-milled to break the dry gel into a network-like thin sheet material, and the particle size of the thin sheet material is controlled to 500-600nm by controlling the ball milling speed and duration; compared with the traditional pyrophosphate, the network-like thin sheet material has a smaller particle size and a larger surface area, which can shorten the ion diffusion particle size, expose more active sites, reduce the material resistance, and is beneficial to NaVP 2 O 7 Release of material specific capacity.
[0011] The technical solution of the present invention is to pulverize NaVP 2 O 7 The precursor material and GO were added to deionized water, and under the action of ultrasound, NaVP 2 O 7 The precursor material is loaded onto GO to form NaVP 2 O 7 Precursor / GO suspension; irregular flake materials of about 500~600nm are loaded on the wrinkled GO, which not only avoids the NaVP 2 O 7 After being sintered, the structural stability can be better maintained during the cycle; the oxygen-containing functional groups on GO are then reduced by hydrothermal reaction to improve the conductivity of the material, and finally a sodium vanadium pyrophosphate / carbon composite material (NaVP 2 O 7 / rGO).
[0012] The technical solution of the present invention controls the calcination temperature and duration of the powder precipitate in an inert atmosphere to cause phosphate to undergo a polymerization reaction to form pyrophosphate. The pyrophosphate has a more stable intrinsic structure, a higher redox potential and better high temperature resistance, and can significantly improve the high temperature resistance of the product, providing a new synthesis path for the preparation of high temperature and high pressure electrode materials.
[0013] The technical solution of the present invention is to NaVP2 O 7 The conductivity of the material has been greatly improved. The sodium vanadium pyrophosphate / carbon composite material (NaVP 2 O 7 / rGO) is applied in sodium ion batteries and shows excellent electrochemical performance. The capacity is maintained at 85.39 mAh g after 1000 cycles under 1C condition. -1 , the cycle attenuation rate is as low as 0.01%. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 The NaVP obtained in Example 1 2 O 7 The morphology of the precursor material observed by scanning electron microscope at 7210 times; Figure 2 The sodium vanadium pyrophosphate / carbon composite material (NaVP 2 O 7 / rGO) morphology at an electron microscope magnification of 9350 times; Figure 3 NaVP obtained in the comparative example 2 O 7 The material was calcined and observed under a scanning electron microscope at 10480 times; Figure 4 The sodium vanadium pyrophosphate / carbon composite material (NaVP 2 O 7 / rGO) XRD diffraction pattern; Figure 5 The sodium vanadium pyrophosphate / carbon composite material (NaVP 2 O 7 / rGO) is used as a positive electrode material in sodium-ion batteries, and the cycling performance diagram at 1C current density. DETAILED DESCRIPTION
[0015] The present invention is further described in detail below in conjunction with the embodiments. The drawings and embodiments of the specification are only used to explain the present invention and do not constitute an improper limitation of the present invention. Example 1
[0016] (1) 0.13 mol Na 2 CO 3 , 0.1molV 2 O 5 、0.2molNH 4 H 2 PO 4, 0.03 mol of citric acid was added to 1 L of deionized water and stirred at 80 ° C for 1 h to obtain a sol, which was placed in an oven for drying to obtain a dry gel. The dry gel and grinding balls were added to a grinding tank at a weight ratio of 1:10, and ground at 700 r / min for 3 h to obtain NaVP 2 O 7 Precursor materials; (2) 500 mg of NaVP2O7 precursor material was added to deionized water and ultrasonically dispersed to form a solution. During the ultrasonic process, 20 mg of GO was added to form a mixed solution. The mixed solution was transferred to a reactor and heated at 160 °C for 10 h to obtain NaVP 2 O 7 Precursor / rGO suspension; (3) NaVP 2 O 7 The precursor / rGO suspension was filtered, washed and dried to obtain a powder precipitate, which was calcined at 800 °C for 10 h in an Ar atmosphere to obtain a sodium vanadium pyrophosphate / carbon composite material (NaVP 2 O 7 / rGO).
[0017] The NaVP obtained in Example 1 2 O 7 The precursor material was characterized by scanning electron microscopy (SEM), and the results of SEM test at 7210 times were as follows: Figure 1 If the material is formed directly by stirring the solution, it is easy to form a large block of material. The technical solution of the present invention obtains a 500-600nm network-like thin sheet material through the steps of forming a sol, a dry gel, and ball milling, which can shorten the ion diffusion path, expose more active sites, reduce the material resistance, and is beneficial to NaVP 2 O 7 The release of material specific capacity. After the ball-milled material is directly calcined, the material morphology and structure are as follows Figure 3 As shown, the material will be sintered. 2 O 7 The / rGO composite material was observed by scanning electron microscopy at a magnification of 9350 times. Figure 2 As shown, the powdered NaVP 2 O 7 The precursor material and GO were hydrothermally reduced and subsequently calcined to form a sodium vanadium pyrophosphate / carbon composite material with a high degree of compositeness (NaVP 2 O 7 / rGO). The irregular flake materials with a diameter of about 500-600 nm are loaded on the wrinkled rGO, which not only avoids the NaVP 2 O7 Even after being sintered, the irregular sheet structure can be evenly dispersed on the rGO. The formation of this structure can not only effectively improve the electrochemical performance of the material, but also better maintain the structural stability during the cycle. Figure 5 As shown in Figure 2, the material maintained a capacity of 85.39 mAh g after 1000 cycles at 1C. -1 The cycle attenuation rate is as low as 0.01%. The XRD diffraction test was carried out on it, and the results are as follows Figure 4 The shown demonstrates the efficient synthesis of the material. Example 2
[0018] (1) 0.1 mol NaCl, 0.1 mol V 2 O 5 、0.2mol(NH 4 ) 2 HPO 4 , 0.03 mol of citric acid was added to 1 L of deionized water and stirred at 80 ° C for 1 h to obtain a sol, which was placed in an oven for drying to obtain a dry gel. The dry gel and grinding balls were added to a grinding tank at a weight ratio of 1:15, and ground at 600 r / min for 5 h to obtain NaVP 2 O 7 Precursor materials; (2) 500 mg of NaVP2O7 precursor material was added to deionized water and ultrasonically dispersed to form a solution. During the ultrasonic process, 30 mg of GO was added to form a mixed solution. The mixed solution was transferred to a reactor and heated at 170 °C for 5 h to obtain NaVP 2 O 7 Precursor / rGO suspension; (3) NaVP 2 O 7 The precursor / rGO suspension was filtered, washed and dried to obtain a powder precipitate, which was calcined at 700 °C in an Ar atmosphere for 10 h to obtain a sodium vanadium pyrophosphate / carbon composite material (NaVP 2 O 7 / rGO). Example 3
[0019] (1) 0.11 mol Na 2 C 2 O 4 、0.1molNH 4 VO 3 、0.2mol(NH 4 ) 2 HPO 4, 0.03 mol of citric acid was added to 1 L of deionized water and stirred at 80 ° C for 1 h to obtain a sol, which was placed in an oven for drying to obtain a dry gel. The dry gel and grinding balls were added to a grinding tank at a weight ratio of 1:20, and ground at 500 r / min for 8 h to obtain NaVP 2 O 7 Precursor materials; (2) 500 mg of NaVP2O7 precursor material was added to deionized water and ultrasonically dispersed to form a solution. During the ultrasonic process, 10 mg of GO was added to form a mixed solution. The mixed solution was transferred to a reactor and heated at 160 °C for 8 h to obtain NaVP 2 O 7 Precursor / rGO suspension; (3) NaVP 2 O 7 The precursor / rGO suspension was filtered, washed and dried to obtain a powder precipitate, which was calcined at 800 °C for 3 h in an Ar atmosphere to obtain a sodium vanadium pyrophosphate / carbon composite material (NaVP 2 O 7 / rGO). Comparative Example
[0020] (1) 0.13 mol Na 2 CO 3 , 0.1molV 2 O 5 、0.2molNH 4 H 2 PO 4 , 0.03 mol of citric acid was added to 1 L of deionized water and stirred at 80 ° C for 1 h to obtain a sol, which was placed in an oven for drying to obtain a dry gel. The dry gel and grinding balls were added to a grinding tank at a weight ratio of 1:10, and ground at 700 r / min for 3 h to obtain NaVP 2 O 7 Precursor materials; (2) NaVP 2 O 7 The precursor material was calcined at 800 °C in an Ar atmosphere for 10 h to obtain NaVP 2 O 7 Material.
[0021]
[0022] The materials prepared in the examples and comparative examples were used as positive electrodes in sodium ion batteries. From the data in Table 1, it can be seen that the electrochemical performance of the material obtained in Example 1 is the best, proving that the conditions used in Example 1 are the best combination of conditions. The comparative example was not composited with wrinkled rGO, and the cycle stability was poor, failing to complete 1000 cycles. This further proves that NaVP 2 O 7 Irregular fragments are conducive to the release of material capacity, rGO and NaVP 2 O 7 The composite of irregular fragment materials is beneficial to maintaining structural stability and improving cycle stability.
Claims
1. A method for synthesizing a sodium vanadium pyrophosphate / carbon composite material, characterized in that: The steps include: (1) adding sodium salt, vanadium-containing compound, ammonium phosphate and citric acid into deionized water, heating and stirring to obtain a sol, drying the sol to obtain a dry gel, and ball-milling the dry gel to obtain a NaVP2O7 precursor material; (2) adding NaVP2O7 precursor material and GO into deionized water, and ultrasonically dispersing them to form a mixed solution; subjecting the mixed solution to a hydrothermal reaction to obtain a NaVP2O7 precursor / rGO suspension; (3) The NaVP2O7 precursor / rGO suspension is filtered, washed, and dried to obtain a powder precipitate, which is then calcined in an inert atmosphere to obtain a sodium vanadium pyrophosphate / carbon composite material.
2. The method for synthesizing the sodium vanadium pyrophosphate / carbon composite material according to claim 1, characterized in that: In the step (1), the sodium salt is one of Na2CO3, NaCl, and Na2C2O4; the vanadium-containing compound is NH4VO3 or V2O5; the ammonium phosphate is NH4H2PO4 or (NH4)2HPO4; the molar ratio of the sodium salt, the vanadium-containing compound, the ammonium phosphate, and the citric acid is 10-13 mol:10 mol:20 mol:3 mol; the ball-to-material ratio is 1:10-20, the rotation speed is 500-700 r / min, and the ball milling time is 3-8 h.
3. The method for synthesizing the sodium vanadium pyrophosphate / carbon composite material according to claim 1, characterized in that: In the step (2), the mass ratio of NaVP2O7 precursor material to GO is 10-30:1; the hydrothermal reaction temperature is 150-170°C; and the heating time is 5-10h.
4. The method for synthesizing the sodium vanadium pyrophosphate / carbon composite material according to claim 1, characterized in that: In the step (3), the calcination temperature is 600°C to 800°C and the calcination time is 8 to 10 hours.
5. An application of a sodium vanadium pyrophosphate / carbon composite material prepared by the synthesis method of the sodium vanadium pyrophosphate / carbon composite material according to any one of claims 1 to 4, characterized in that: The sodium vanadium pyrophosphate / carbon composite material is used as a positive electrode material for a sodium ion battery.
Citation Information
Patent Citations
High-magnification sodium-ion battery composite cathode material and preparation method
CN104362309A
Sodium vanadium pyrophosphate / carbon composite positive electrode material, and preparation and application thereof
CN107017398A
Heteroatom-doped graphene-based sodium vanadium phosphate composite nanometer material of sodium ion positive electrode material
CN109616651A
Reduced graphene oxide modified sodium vanadium oxyfluoride phosphate positive electrode material as well as preparation method and application thereof
CN117446779A
A process for the preparation of sodium vanadium phosphate
IN202211053978A