Biomass-based hard carbon material as well as preparation method and application thereof
By mixing biomass raw materials with nitrogen-containing biomass for heat treatment and using nitrogen-doped carbonization process, the problems of unstable supply and insufficient performance of hard carbon materials were solved, and high-performance nitrogen-doped hard carbon materials were prepared, which improved the electrochemical performance of sodium-ion batteries.
Patent Information
- Application Number
- CN202410989469.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The supply of precursors for existing hard carbon materials is unstable and costly. Furthermore, the hard carbon materials prepared from them have low specific capacity, low initial coulombic efficiency, and poor cycle performance, making it difficult to meet the commercialization requirements of sodium-ion batteries.
High-performance nitrogen-doped hard carbon materials are prepared by mixing biomass raw materials with nitrogen-containing biomass raw materials and through heat treatment and nitrogen doping carbonization processes. The oxygen-containing groups generate pores and nitrogen doping increases the active sites for sodium ion storage, promotes electron ion diffusion, and reduces side reactions.
The discharge specific capacity, first-cycle coulombic efficiency, and cycle stability of the hard carbon material were improved. The prepared biomass-based hard carbon material exhibited excellent electrochemical performance in sodium-ion batteries, with a discharge specific capacity of up to 356.2 mAh/g, a first-cycle coulombic efficiency of 92.3%, and a capacity retention rate of 91.7% after 1000 cycles.
Smart Images

Figure CN118929626A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of hard carbon materials, and in particular refers to a biomass-based hard carbon material and a preparation method and application thereof. Background Art
[0002] The complementarity between sodium-ion batteries and lithium-ion batteries gives them broad application prospects. The development of low-cost, high-performance electrode materials is the key to the commercial application of sodium-ion batteries. Hard carbon materials are the most promising negative electrode materials for sodium-ion batteries for commercial application, but their current development status is still far from large-scale industrialization.
[0003] Hard carbon materials have a larger graphite layer spacing, more disordered structures and closed pore structures, which are conducive to the storage and diffusion of sodium ions. The structure and properties of hard carbon materials mainly depend on the precursors and the corresponding carbonization process, among which the precursors mainly include biomass-based, synthetic polymers and fossil fuel-based precursors. Synthetic polymers are relatively expensive, fossil fuel-based precursors have more impurities and poor product performance, and synthetic polymers and fossil fuel-based precursors generally need to be cross-linked and oxidized first to give them a non-graphite structure. These processes use catalysts, oxidants, hydrogen and other additives, which increase production costs and produce toxic substances, bringing greater environmental pressure. The hard carbon produced by the biomass-based route has better performance, a wide range of material sources, and relatively appropriate costs. It is currently the choice of major production companies.
[0004] The earliest companies to deploy hard carbon materials were mainly Japanese companies, among which Kuraray was the representative company. Kuraray of Japan uses biomass material coconut shell as hard carbon precursor, which is processed by carbonization, crushing, alkali staining, heat treatment purification and CVD treatment. The process is relatively complicated, among which the CVD treatment process is more difficult. The price of Kuraray hard carbon products is as high as 200,000 yuan / ton. The domestic company Bester Hard Carbon uses biomass materials such as starch as raw materials, and prepares hard carbon through modification, cracking and condensation, carbonization and surface modification. The process is also relatively complicated.
[0005] The biggest problem with using biomass coconut shell as a hard carbon precursor is that the output is limited by the output of coconuts, the domestic raw material supply is insufficient, and it is overly dependent on imports. The main problem with using starch as a hard carbon precursor is that the process cost is high, and additional additives such as cross-linking agents or hydrogenation modification are required. Other biomass raw materials such as wood, bamboo, fruit shells, rice husks, straw, etc. are difficult to ensure stable supply and batch consistency, and the prepared hard carbon materials have problems such as low specific capacity, low first coulomb efficiency, and poor cycle performance. Patent CN113206246A discloses a method for preparing a biomass hard carbon negative electrode material for a sodium ion battery, using wood as a biomass carbon source, ultrasonically washing with deionized water, and drying to obtain a biomass precursor. The final performance of the material lacks competitiveness, and it shows a reversible specific capacity of 258.1mAh / g after 100 cycles at a current density of 30mA / g, and the capacity retention rate is 85%. Therefore, improving the specific capacity, first coulomb efficiency and cycle stability of the material has become another key issue for hard carbon materials. Summary of the invention
[0006] In response to the technical problems of hard carbon material precursor selection, preparation process, low first coulombic efficiency and poor cycle performance of hard carbon materials, the present invention provides a biomass-based hard carbon material and a preparation method and application thereof.
[0007] To achieve the above object, the technical solution of the present invention is implemented as follows: A method for preparing a biomass-based hard carbon material, comprising the following steps: (1) ball-milling the biomass raw material and the nitrogen-containing biomass raw material to uniformly obtain a composite precursor; (2) heat treating the composite precursor obtained in step (1) in an inert atmosphere to obtain a pyrolysis product; (3) subjecting the pyrolysis product obtained in step (2) to a second heat treatment in an inert atmosphere to obtain a nitrogen-doped carbide; (4) Grinding and crushing the nitrogen-doped carbide obtained in step (3), washing, vacuum drying, crushing and screening to obtain a biomass-based hard carbon material.
[0008] In the above step (1), the biomass raw material is one or more of xanthan gum, guar gum, carrageenan, pectic acid, pectin, xylan, konjac glucomannan, salicylic acid, wattle bark tannin, gum arabic, larch tannin, chestnut tannin, tara tannin, quebracho tannin, commercial peach gum and bladder gum.
[0009] In the above step (1), the nitrogen-containing biomass raw material is chitin, chitosan, amino acid, straw, distiller's grains, mushroom sticks or nitrogen-containing agricultural waste.
[0010] More preferably, the nitrogen-containing biomass raw material in step (1) is chitin or chitosan.
[0011] In the above step (1), the mass ratio of the biomass raw material to the nitrogen-containing biomass raw material is (1-20):1; and the ball milling time is 1-3h.
[0012] The heat treatment in the above step (2) refers to heating the temperature to 400-700°C at a heating rate of 0.5-10°C / min and keeping the temperature for 0.5-10h.
[0013] The second heat treatment in the above step (3) refers to heating the temperature to 1000-1800°C at a heating rate of 2-10°C / min and keeping the temperature for 1-8h.
[0014] The washing process in the above step (4) is as follows: mixing and stirring the ground nitrogen-doped carbide with an acidic solution, filtering and washing until neutral, and then washing with ethanol; and sieving to pass through a 200-1000 mesh sieve.
[0015] The acidic solution is one of hydrochloric acid, sulfuric acid, nitric acid, citric acid and acetic acid; the concentration of the acidic solution is 0.1-6 mol / L; the solid-liquid ratio of the ground nitrogen-doped carbide to the acidic solution is 0.005-0.1 g / mL.
[0016] The biomass-based hard carbon material prepared by the above preparation method.
[0017] The above-mentioned biomass-based hard carbon material is used as a hard carbon negative electrode material in sodium ion batteries.
[0018] Commercial biomass raw materials are used as hard carbon precursors, and high-performance nitrogen-doped hard carbon materials are prepared through a simple and easily scalable process. The biomass raw materials used in the present invention are easy to obtain and preserve, with a stable supply and low cost, which can ensure the low cost, stability and consistency of the hard carbon precursor. The present invention selects biomass industrial raw materials containing a large number of oxygen-containing groups hydroxyl (-OH) and carboxyl (-COOH) as hard carbon precursors. The oxygen-containing groups will be converted into H2O and CO2 during the pyrolysis process. When the gas escapes, a large number of pores will be generated in the carbon matrix, which can promote the storage and diffusion of sodium ions and the penetration of electrolytes. The present invention uses nitrogen-containing biomass raw materials to nitrogen-dope and carbon-coat hard carbon materials, which can increase the active sites for sodium ion storage, promote the efficient diffusion of electronic ions, slow down the side reactions of hard carbon and electrolytes, and increase the coulombic efficiency of hard carbon materials.
[0019] The present invention has the following beneficial effects: 1. The present invention uses commercial biomass raw materials as hard carbon precursors and nitrogen-containing biomass raw materials as nitrogen doping materials. The raw materials are widely available, have a stable supply, are low-cost, are easy to obtain and preserve, and can ensure the low cost, stability and consistency of the hard carbon precursor.
[0020] 2. The present invention selects biomass raw materials containing a large number of oxygen-containing groups (such as hydroxyl (-OH), carboxyl (-COOH)) as hard carbon precursors. The oxygen-containing groups will generate gases such as H2O and CO2 during the pyrolysis process. When the gases escape, a large number of pores will be generated in the carbon matrix, which can promote the storage and diffusion of sodium ions and the penetration of electrolytes, which is beneficial to the improvement of the electrochemical performance of sodium ion batteries.
[0021] 3. The present invention uses nitrogen-containing biomass materials such as chitin or chitosan to nitrogen-dope hard carbon materials, which can cause a large number of defects in the hard carbon, increase the active sites for sodium ion storage, and promote the efficient diffusion of electron ions; at the same time, the nitrogen-containing biomass precursor is pyrolyzed to generate amorphous carbon coated on the surface of the hard carbon, which can greatly reduce the side reactions between the hard carbon and the electrolyte during the charge and discharge process and increase the coulombic efficiency of the hard carbon material.
[0022] 4. The present invention selects biomass raw materials containing a large number of oxygen groups as hard carbon precursors, and this preparation method is combined with the subsequent nitrogen doping and carbon coating process, which is conducive to the application of hard carbon materials in sodium ion batteries. The discharge capacity, first-week coulomb efficiency and cycle capacity retention rate are improved. When the hard carbon material prepared in Example 1 is used as the negative electrode material of the sodium ion battery, the electrochemical performance is the best, the discharge capacity can reach 356.2mAh / g, the first-week coulomb efficiency is 92.3% and the 1000 times 1C cycle capacity retention rate is maintained at 91.7%. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 This is the XRD spectrum of the hard carbon material prepared in Example 1 of the present invention.
[0025] Figure 2 This is a scanning electron microscope image of the hard carbon material prepared in Example 1 of the present invention.
[0026] Figure 3 This is the first cycle charge and discharge curve of the hard carbon material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0027] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of xanthan gum, add chitosan in a mass ratio of xanthan gum to nitrogen-containing biological raw material of 1:1, and ball mill for 1 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 400°C at a rate of 0.5°C / min in a nitrogen atmosphere, and keeping it at that temperature for 0.5h, cooling it to room temperature, and taking it out to obtain a pyrolysis product; (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1000°C at a rate of 2°C / min in a nitrogen atmosphere, keeping it at that temperature for 8 hours, cooling it to room temperature, and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 0.1 mol / L hydrochloric acid is added at a solid-liquid ratio of 0.1 g / mL, the mixture is mixed and stirred at 30°C for 6 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 50°C for 8 h, crushed with a jet mill, and sieved through an 800-mesh sieve to obtain a biomass-based hard carbon material.
[0029] Figure 1 : This is the XRD pattern of the hard carbon material prepared in Example 1 of the present invention. As can be seen from the figure, the XRD pattern of the material shows a typical XRD pattern of hard carbon materials, and the two peaks at 22° and 44° correspond to the (002) and (101) planes of the graphite-like structure, respectively.
[0030] Figure 2 This is a scanning electron microscope image of the hard carbon material prepared in Example 1 of the present invention. It can be seen from the figure that the surface and interior of the material contain a large number of pores to form a hierarchical porous structure, which can promote the storage and diffusion of sodium ions and the penetration of electrolytes.
[0031] Figure 3This is the first week charge and discharge curve of the hard carbon material prepared in Example 1 of the present invention. It can be seen from the figure that the material discharge and sodium storage has both slope discharge and platform discharge stages, and the platform discharge stage is longer, indicating that the material has good cycle stability. At 30mA / g, the initial discharge specific capacity is 356.2 mAh / g, the initial charge specific capacity is 328.8 mAh / g, and the first coulomb efficiency is 92.3%, which is a hard carbon material with excellent electrochemical performance.
[0032] Example 2 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of guar gum, add chitosan according to the mass ratio of guar gum to nitrogen-containing biological raw material of 3:1, and ball mill for 2 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in the constant temperature zone of a tube furnace, heating it to 600°C at a rate of 5°C / min in a nitrogen atmosphere and keeping it at that temperature for 3 h, cooling it to room temperature and taking it out to obtain a pyrolysis product; (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1100° C. at a rate of 5° C. / min in a nitrogen atmosphere, keeping it at that temperature for 2 h, cooling it to room temperature, and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 1 mol / L sulfuric acid is added at a solid-liquid ratio of 0.01 g / mL, the mixture is mixed and stirred at 50°C for 10 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 60°C for 10 h, crushed with a jet mill, and sieved through a 200-mesh sieve to obtain a biomass-based hard carbon material.
[0033] Example 3 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of carrageenan, add chitosan in a mass ratio of carrageenan to nitrogen-containing biological raw material of 5:1, and mix by ball milling for 3 h to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in the constant temperature zone of a tube furnace, heating it to 500°C at 4°C / min in a nitrogen atmosphere, keeping it at that temperature for 6 hours, cooling it to room temperature, and taking it out to obtain a pyrolysis product; (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1200°C at 6°C / min in a nitrogen atmosphere, keeping it at that temperature for 4 hours, cooling it to room temperature and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 2 mol / L nitric acid is added at a solid-liquid ratio of 0.008 g / mL, the mixture is mixed and stirred at 60°C for 12 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 70°C for 12 h, crushed with a jet mill, and sieved through a 500-mesh sieve to obtain a biomass-based hard carbon material.
[0034] Example 4 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of pectin acid, add chitosan according to the mass ratio of pectin acid to nitrogen-containing biological raw material of 6:1, and ball mill for 2 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 700°C at a rate of 6°C / min in a nitrogen atmosphere, and keeping it at that temperature for 10 h. After cooling it to room temperature, the crucible was taken out to obtain a pyrolysis product. (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1300° C. at 8° C. / min in a nitrogen atmosphere, keeping it at that temperature for 7 h, cooling it to room temperature, and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 6 mol / L citric acid is added at a solid-liquid ratio of 0.006 g / mL, the mixture is mixed and stirred at 100°C for 24 hours, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 60°C for 10 hours, crushed with a jet mill, and sieved through a 500-mesh sieve to obtain a biomass-based hard carbon material.
[0035] Example 5 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of pectin, add chitosan according to the mass ratio of pectin to nitrogen-containing biological raw material of 10:1, and ball mill for 3 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 700°C at a rate of 10°C / min in a nitrogen atmosphere, and keeping it at that temperature for 10 h. After cooling it to room temperature, the crucible was taken out to obtain a pyrolysis product. (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1100° C. at a rate of 8° C. / min in a nitrogen atmosphere, keeping it at that temperature for 8 h, cooling it to room temperature, and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 1 mol / L acetic acid is added at a solid-liquid ratio of 0.01 g / mL, the mixture is mixed and stirred at 50°C for 10 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 60°C for 10 h, crushed with a jet mill, and sieved through a 500-mesh sieve to obtain a biomass-based hard carbon material.
[0036] Example 6 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of xylan, add chitosan according to the mass ratio of xylan to nitrogen-containing biological raw material of 17:1, and ball mill for 2 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 600°C at a rate of 2°C / min in a nitrogen atmosphere, and keeping it at that temperature for 3 h. After cooling it to room temperature, the crucible was taken out to obtain a pyrolysis product. (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1600°C at a rate of 10°C / min in a nitrogen atmosphere, keeping it at that temperature for 5 hours, cooling it to room temperature and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 1 mol / L hydrochloric acid is added at a solid-liquid ratio of 0.01 g / mL, the mixture is mixed and stirred at 50°C for 10 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 60°C for 10 h, crushed with a jet mill, and sieved through a 500-mesh sieve to obtain a biomass-based hard carbon material.
[0037] Example 7 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of konjac glucomannan, add chitosan according to the mass ratio of konjac glucomannan to nitrogen-containing biological raw material of 20:1, and ball mill for 2 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 600°C at a rate of 10°C / min in a nitrogen atmosphere, and keeping it at that temperature for 3 h. After cooling it to room temperature, the crucible was taken out to obtain a pyrolysis product. (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1800°C at 4°C / min in a nitrogen atmosphere, keeping it at that temperature for 1 hour, cooling it to room temperature and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 6 mol / L hydrochloric acid is added at a solid-liquid ratio of 0.005 g / mL, the mixture is mixed and stirred at 50°C for 24 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 90°C for 24 h, crushed with a jet mill, and sieved through a 1000 mesh sieve to obtain a biomass-based hard carbon material.
[0038] Example 8 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of salicylic acid, add chitosan in a mass ratio of salicylic acid to nitrogen-containing biological raw material of 1:1, and ball mill for 1 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in the constant temperature zone of a tube furnace, heating it to 600°C at a rate of 5°C / min in a nitrogen atmosphere, keeping it at that temperature for 0.5 h, cooling it to room temperature, and taking it out to obtain a pyrolysis product; (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1000°C at a rate of 5°C / min in a nitrogen atmosphere, keeping it at that temperature for 8 hours, cooling it to room temperature, and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 0.1 mol / L hydrochloric acid is added at a solid-liquid ratio of 0.1 g / mL, the mixture is mixed and stirred at 30°C for 6 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 50°C for 8 h, crushed with a jet mill, and sieved through an 800-mesh sieve to obtain a biomass-based hard carbon material.
[0039] Example 9 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of tannin extract from the bark of wattle, add chitosan in a mass ratio of 1:1 between tannin extract from the bark of wattle and nitrogen-containing biological raw material, and ball mill for 1 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in the constant temperature zone of a tube furnace, heating it to 400°C at a rate of 5°C / min in a nitrogen atmosphere, keeping it at that temperature for 0.5 h, cooling it to room temperature, and taking it out to obtain a pyrolysis product; (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1000°C at a rate of 5°C / min in a nitrogen atmosphere, keeping it at that temperature for 8 hours, cooling it to room temperature, and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 0.1 mol / L hydrochloric acid is added at a solid-liquid ratio of 0.1 g / mL, the mixture is mixed and stirred at 30°C for 6 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 50°C for 8 h, crushed with a jet mill, and sieved through an 800-mesh sieve to obtain a biomass-based hard carbon material.
[0040] Example 10 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of gum arabic, add chitosan in a mass ratio of gum arabic to nitrogen-containing biological raw material of 1:1, and ball mill for 1 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in the constant temperature zone of a tube furnace, heating it to 400°C at a rate of 10°C / min in a nitrogen atmosphere, keeping it at that temperature for 0.5 h, cooling it to room temperature, and taking it out to obtain a pyrolysis product; (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1000°C at a rate of 10°C / min in a nitrogen atmosphere, keeping it at that temperature for 8 hours, cooling it to room temperature and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 0.1 mol / L hydrochloric acid is added at a solid-liquid ratio of 0.1 g / mL, the mixture is mixed and stirred at 30°C for 6 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 50°C for 8 h, crushed with a jet mill, and sieved through an 800-mesh sieve to obtain a biomass-based hard carbon material.
[0041] Embodiment 11 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of larch tannin extract, add chitosan according to the mass ratio of larch tannin extract to nitrogen-containing biological raw material of 1:1, and ball mill for 1 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in the constant temperature zone of a tube furnace, heating it to 400°C at a rate of 5°C / min in a nitrogen atmosphere, keeping it at that temperature for 0.5 h, cooling it to room temperature, and taking it out to obtain a pyrolysis product; (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1000°C at a rate of 5°C / min in a nitrogen atmosphere, keeping it at that temperature for 8 hours, cooling it to room temperature, and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 0.1 mol / L hydrochloric acid is added at a solid-liquid ratio of 0.1 g / mL, the mixture is mixed and stirred at 30°C for 6 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 50°C for 8 h, crushed with a jet mill, and sieved through an 800-mesh sieve to obtain a biomass-based hard carbon material.
[0042] Example 12 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of chestnut tannin extract, add chitosan in a mass ratio of chestnut tannin extract to nitrogen-containing biological raw material of 1:1, and ball mill for 1 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in the constant temperature zone of a tube furnace, heating it to 400°C at a rate of 5°C / min in a nitrogen atmosphere, keeping it at that temperature for 0.5 h, cooling it to room temperature, and taking it out to obtain a pyrolysis product; (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1000°C at a rate of 5°C / min in a nitrogen atmosphere, keeping it at that temperature for 8 hours, cooling it to room temperature, and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 0.1 mol / L hydrochloric acid is added at a solid-liquid ratio of 0.1 g / mL, the mixture is mixed and stirred at 30°C for 6 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 50°C for 8 h, crushed with a jet mill, and sieved through an 800-mesh sieve to obtain a biomass-based hard carbon material.
[0043] Embodiment 13 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of tara tannin extract, add chitosan in a mass ratio of tara tannin extract to nitrogen-containing biological raw material of 1:1, and ball mill for 1 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in the constant temperature zone of a tube furnace, heating it to 400°C at 6°C / min in a nitrogen atmosphere, keeping it at that temperature for 0.5h, cooling it to room temperature, and taking it out to obtain a pyrolysis product; (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1000°C at 6°C / min in a nitrogen atmosphere, keeping it at that temperature for 8 hours, cooling it to room temperature and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 0.1 mol / L hydrochloric acid is added at a solid-liquid ratio of 0.1 g / mL, the mixture is mixed and stirred at 30°C for 6 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 50°C for 8 h, crushed with a jet mill, and sieved through an 800-mesh sieve to obtain a biomass-based hard carbon material.
[0044] Embodiment 14 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of quebracho tannin extract, add chitosan in a mass ratio of quebracho tannin extract to nitrogen-containing biological raw material of 1:1, and ball mill for 1 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in the constant temperature zone of a tube furnace, heating it to 400°C at 7°C / min in a nitrogen atmosphere, keeping it at that temperature for 0.5 h, cooling it to room temperature, and taking it out to obtain a pyrolysis product; (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1000° C. at 7° C. / min in a nitrogen atmosphere, keeping it at that temperature for 8 h, cooling it to room temperature, and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 0.1 mol / L hydrochloric acid is added at a solid-liquid ratio of 0.1 g / mL, the mixture is mixed and stirred at 30°C for 6 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 50°C for 8 h, crushed with a jet mill, and sieved through an 800-mesh sieve to obtain a biomass-based hard carbon material.
[0045] Embodiment 15 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of commercial peach gum, add chitosan according to the mass ratio of commercial peach gum to nitrogen-containing biological raw material of 1:1, and ball mill for 1 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in the constant temperature zone of a tube furnace, heating it to 400°C at 8°C / min in a nitrogen atmosphere, keeping it at that temperature for 0.5h, cooling it to room temperature, and taking it out to obtain a pyrolysis product; (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1000° C. at a rate of 8° C. / min in a nitrogen atmosphere, keeping it at that temperature for 8 h, cooling it to room temperature, and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 0.1 mol / L hydrochloric acid is added at a solid-liquid ratio of 0.1 g / mL, the mixture is mixed and stirred at 30°C for 6 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 50°C for 8 h, crushed with a jet mill, and sieved through an 800-mesh sieve to obtain a biomass-based hard carbon material.
[0046] Example 16 The preparation method of the biomass-based hard carbon material of this embodiment comprises the following steps: (1) Take 100 g of bladder gel, add chitosan in a mass ratio of 1:1 between bladder gel and nitrogen-containing biological raw material, and ball mill for 1 h to mix evenly to obtain a composite precursor; (2) placing the composite precursor into a corundum crucible, placing it in the constant temperature zone of a tube furnace, heating it to 400°C at a rate of 9°C / min in a nitrogen atmosphere, keeping it at that temperature for 0.5 h, cooling it to room temperature, and taking it out to obtain a pyrolysis product; (3) crushing the pyrolysis product obtained in step (2) into powder, then putting it into a corundum crucible, placing it in a constant temperature zone of a tube furnace, heating it to 1000° C. at a rate of 9° C. / min in a nitrogen atmosphere, keeping it at that temperature for 8 h, cooling it to room temperature, and taking it out to obtain nitrogen-doped carbide; (4) The nitrogen-doped carbide obtained in step (3) is ground into fine powder using a grinder, 0.1 mol / L hydrochloric acid is added at a solid-liquid ratio of 0.1 g / mL, the mixture is mixed and stirred at 30°C for 6 h, filtered and washed until the pH value is 7, then washed with ethanol, vacuum dried at 50°C for 8 h, crushed with a jet mill, and sieved through an 800-mesh sieve to obtain a biomass-based hard carbon material.
[0047] Application Examples The biomass-based hard carbon materials prepared in Examples 1-16 were used as negative electrode materials for sodium ion batteries, and half-cells were assembled for testing. The hard carbon materials in the above examples were slurried according to the ratio of hard carbon material: sodium carboxymethyl cellulose (CMC): conductive carbon black (Super-p) = 9:0.5:0.5 (weight ratio). The slurry was adjusted with deionized water, coated on aluminum foil and dried in a vacuum drying oven for 12 hours to form an electrode sheet. A glass fiber separator and metallic sodium were used as the negative electrode sheet. Commercially available sodium ion electrolyte was used to assemble CR2025 button batteries in an argon atmosphere. The charge and discharge voltage range was 0-2.0V. The charge and discharge test was carried out at a current density of 30mA / g in the first week. The cycle performance test was carried out at a rate of 1C. The results are shown in Table 1.
[0048] Table 1 Electrochemical test results of Examples 1-16 As can be seen from the above table, the hard carbon negative electrode material prepared by the present invention has excellent discharge specific capacity, first-week efficiency and cycle performance when used in sodium ion batteries. When the hard carbon material prepared in Example 1 is used as the negative electrode material of the sodium ion battery, the electrochemical performance is the best, the discharge specific capacity can reach 356.2mAh / g, the first-week coulomb efficiency is 92.3%, and the capacity retention rate of 1000 1C cycles is maintained at 91.7%. The present invention preferably uses biomass industrial raw materials with a large number of oxygen-containing groups as hard carbon precursors, and the prepared hard carbon material has a large number of pores, which can promote sodium ion storage and diffusion and electrolyte penetration; the present invention performs nitrogen doping and carbon coating on the hard carbon material, which can increase the sodium ion storage active sites, promote efficient diffusion of electron ions, slow down the side reactions of hard carbon and electrolyte, and increase the coulomb efficiency of hard carbon materials. Therefore, the hard carbon negative electrode material prepared by the present invention shows excellent performance in sodium ion batteries.
[0049] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a biomass-based hard carbon material, characterized in that: Here are the steps: (1) ball-milling the biomass raw material and the nitrogen-containing biomass raw material to uniformly obtain a composite precursor; (2) heat treating the composite precursor obtained in step (1) in an inert atmosphere to obtain a pyrolysis product; (3) subjecting the pyrolysis product obtained in step (2) to a second heat treatment in an inert atmosphere to obtain a nitrogen-doped carbide; (4) Grinding and crushing the nitrogen-doped carbide obtained in step (3), washing, vacuum drying, crushing and screening to obtain a biomass-based hard carbon material.
2. The method for preparing a biomass-based hard carbon material according to claim 1, characterized in that: In the step (1), the biomass raw material is one or more of xanthan gum, guar gum, carrageenan, pectin acid, pectinose, xylan, konjac glucomannan, salicylic acid, wattle bark tannin, gum arabic, larch tannin, chestnut tannin, tara tannin, quebracho tannin, commercial peach gum and bladder gum.
3. The method for preparing a biomass-based hard carbon material according to claim 2, characterized in that: The nitrogen-containing biomass raw material in step (1) is chitin, chitosan, amino acid, straw, distiller's grains, mushroom sticks or nitrogen-containing agricultural waste.
4. The method for preparing a biomass-based hard carbon material according to claim 3, characterized in that: In the step (1), the mass ratio of the biomass raw material to the nitrogen-containing biomass raw material is (1-20):1; and the ball milling time is 1-3 hours.
5. The method for preparing a biomass-based hard carbon material according to claim 4, characterized in that: The heat treatment in step (2) refers to heating the temperature to 400-700°C at a heating rate of 0.5-10°C / min and keeping the temperature for 0.5-10h.
6. The method for preparing a biomass-based hard carbon material according to claim 5, characterized in that: The second heat treatment in step (3) refers to heating the temperature to 1000-1800°C at a heating rate of 2-10°C / min and keeping the temperature for 1-8h.
7. The method for preparing a biomass-based hard carbon material according to claim 6, characterized in that: The washing process in step (4) is as follows: mixing and stirring the ground nitrogen-doped carbide with an acidic solution, filtering and washing until neutral, and then washing with ethanol; Sieve through 200-1000 mesh sieve.
8. The method for preparing a biomass-based hard carbon material according to claim 7, characterized in that: The acidic solution is one of hydrochloric acid, sulfuric acid, nitric acid, citric acid and acetic acid; the concentration of the acidic solution is 0.1-6 mol / L; the solid-liquid ratio of the ground nitrogen-doped carbide to the acidic solution is 0.005-0.1 g / mL.
9. A biomass-based hard carbon material prepared by the preparation method according to any one of claims 1 to 8.
10. The biomass-based hard carbon material according to claim 9 is used as a hard carbon negative electrode material in a sodium ion battery.
Citation Information
Patent Citations
Nitrogen-doped hard carbon material and preparation method and application thereof
CN113493195A
Porous hard carbon negative electrode material based on asphalt as well as preparation method and application of porous hard carbon negative electrode material
CN115676804A
Preparation method of hard carbon negative electrode material, negative electrode plate and sodium ion battery
CN117756084A
High-carbon-yield nitrogen-doped sodium ion battery hard carbon negative electrode material and preparation method thereof
CN118026145A
Composite hard carbon material, preparation method therefor, and use thereof
WO2024109849A1