Nano-graphene and preparation method thereof, nano-graphene polyurethane coating and preparation method and application of nano-graphene polyurethane coating
By preparing nanographene and combining it with polyurethane, the problem of slow heat dissipation of electric vehicle motor controllers is solved, and more efficient thermal management is achieved, which is suitable for mass production applications of electric vehicles.
Patent Information
- Application Number
- CN202410974905.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
AI Technical Summary
The existing electric vehicle motor controllers do not have good heat dissipation effect under high load conditions, resulting in excessive temperature and affecting efficiency. The size of traditional graphene microsheets is too large, resulting in uneven dispersion and poor density. The existing technology does not fully explore the nano-size. Heat dissipation effect.
Nanographene is prepared through homogenization and sand grinding technology, combined with polyurethane coating, and high-pressure microjet treatment and negative pressure stirring technology are used to prepare nanographene polyurethane coating and spray it on the motor controller to improve heat dissipation performance.
It significantly improves the heat dissipation performance of the motor controller, solves the problems of excessive size and uneven dispersion of traditional graphene, and realizes more efficient thermal management, which is suitable for mass production applications of electric vehicles.
Smart Images

Figure CN118929643A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of polyurethane heat dissipation coatings, and more specifically, relates to nano-graphene and a preparation method thereof, and nano-graphene polyurethane coating and a preparation method and application thereof. Background Art
[0002] In electric vehicles, the function of the motor controller is to convert the electric energy stored in the power battery into the electric energy required to drive the motor according to the gear position, accelerator, brake and other instructions to control the start-up, forward and backward speed, climbing strength and other driving conditions of the electric vehicle. It is one of the key components of electric vehicles. When the temperature of the controller itself exceeds a certain temperature, the output current is automatically reduced, and there is a maximum temperature limit protection. Generally speaking, when the electric vehicle is overloaded or climbing, the controller output current is too large, resulting in excessive internal temperature. Once the temperature limit is exceeded, the output efficiency of the electric vehicle will be greatly reduced. Therefore, the economical and fast heat dissipation method of the controller becomes a problem. Chemically produced graphene has poor heat dissipation due to structural defects. Traditional graphene microsheets have large sheet diameters and thicknesses, which make the filler poorly dispersed in the resin, resulting in poor continuity and density of the coating, and also reduce heat dissipation performance.
[0003] The prior art only mentions the combination of resin and graphene, but does not examine the heat dissipation effect of graphene sheets at the nanometer scale. There is also a lack of targeted case applications and characterization of nanographene actually used in heat dissipation coatings. Therefore, it is urgent to propose a nanographene and preparation method and a graphene polyurethane heat dissipation coating and application. Summary of the invention
[0004] The purpose of the present invention is to address the deficiencies of the prior art and to provide a nanographene and a preparation method thereof and a nanographene polyurethane coating and a preparation method and application thereof. The present invention focuses on preparing graphene with a nanometer sheet diameter and a thin thickness, prepares nanographene through homogenization and sand milling technology, and a multi-stage sorting process, and characterizes it, and can achieve mass production.
[0005] In order to achieve the above object, the present invention provides a method for preparing nanographene in a first aspect, the preparation method comprising the following steps:
[0006] S1: Mixing and stirring expanded graphite microsheets, water and an organic solvent to obtain a first mixed material; high-pressure homogenization treatment of the first mixed material to peel off the expanded graphite microsheets in the first mixed material to obtain a slurry;
[0007] S2: sand-milling and filter-pressing the mixture to obtain a filter cake;
[0008] S3: mixing the filter cake with water and the first dispersant and stirring them uniformly to obtain a second mixed material; and subjecting the second mixed material to a high-pressure microfluidization treatment to obtain a dispersion of the nano-graphene.
[0009] According to the present invention, preferably, in step S1:
[0010] The organic solvent is at least one of N-methylpyrrolidone, DMF, ethanol and water;
[0011] The speed of mixing and stirring is 950-1050r / min;
[0012] The first mixed material is treated with high pressure homogenization for 1-5 times; the working pressure of the high pressure homogenization is 20-30 MPa, and the feed rate is 0.1-1 L / s.
[0013] According to the present invention, preferably, in step S2:
[0014] The equipment used for the sand milling process includes a sand mill; the rotation speed of the sand mill is 1400-1600r / min; the sand milling process lasts for 0.8-1.2h; the particle size of the solid material obtained by the sand milling process is D50 less than 5 microns;
[0015] The solid content of the filter cake is 14-18%, which provides an accurate solid content ratio for subsequent high-pressure microfluidization to achieve the best particle size effect. The equipment used for the filter press treatment includes a plate and frame filter press.
[0016] According to the present invention, preferably, in step S3:
[0017] The mass ratio of the filter cake, water and the first dispersant is (900-1100):(2500-5500):(15-25);
[0018] The speed of mixing and stirring is 950-1050r / min;
[0019] The second mixed material is treated with high-pressure microfluidization for 8-12 times; the working pressure of the high-pressure microfluidization treatment is 120-150 MPa, the flow rate is 100-200 L / h, and the working temperature is 60-70°C.
[0020] The solid content of the nano-graphene dispersion is 2-4.5%.
[0021] The second aspect of the present invention provides a dispersion of nano-graphene prepared by the method for preparing nano-graphene.
[0022] The third aspect of the present invention provides a nano-graphene polyurethane coating, which comprises the following components: a polyurethane prepolymer, an additive and a dispersion of the nano-graphene.
[0023] According to the present invention, preferably, the coating comprises the following components in parts by weight: 15-75 parts of polyurethane prepolymer, 8-10 parts of auxiliary agent and 5-45 parts of nanographene dispersion.
[0024] According to the present invention, preferably, the auxiliary agent includes the following components: a second dispersant, a defoamer, a thixotropic agent, a stannous octoate catalyst and an oxazolidine latent curing agent; the ratio of the total mass of the second dispersant, the defoamer, the thixotropic agent and the stannous octoate catalyst to the total mass of the oxazolidine latent curing agent is (3.5-4.5): (4.5-5.5).
[0025] The fourth aspect of the present invention provides a method for preparing the nano-graphene polyurethane coating, which comprises: mixing the polyurethane prepolymer, the additive and the dispersion of nano-graphene, stirring them uniformly under negative pressure, and filtering to obtain the nano-graphene polyurethane coating (a gray-black uniform slurry).
[0026] According to the present invention, preferably, the temperature of negative pressure stirring is 55-65°C, the pressure of negative pressure stirring is -0.100 to -0.090MPa, and the speed of negative pressure stirring is 950-1050r / min. The equipment used for negative pressure stirring includes a vacuum planetary mixer.
[0027] A fifth aspect of the present invention provides the use of the nano-graphene polyurethane coating as a heat dissipation coating for a motor controller.
[0028] In the present invention, as a preferred embodiment, the nano-graphene polyurethane coating is sprayed on the motor controller. Spraying is carried out with a manual spray gun, and the material must be discharged evenly and atomized well before spraying. The nozzle is about 200mm away from the substrate and is swept evenly from left to right. Ensure that the coating achieves good coverage on the substrate. The wet film thickness is about 60um, and the dry film thickness is about 10um. After spraying, it should be left to stand for one minute before baking to achieve better coating flatness and prevent blistering. Curing method: bake at 120°C for 15 minutes.
[0029] The beneficial effects of the technical solution of the present invention are as follows:
[0030] The present invention focuses on preparing graphene with a nanometer sheet diameter and a thin thickness. Nanographene is prepared through homogenization and sand grinding technology and a multi-stage sorting process, and is characterized, and can be mass-produced.
[0031] The nanographene polyurethane coating of the present invention has outstanding heat dissipation performance, mainly because the original micron-sized graphene is nanosized, the particle size of the filler is reduced, the surface area is increased, and the emissivity is relatively improved, solving the problems of existing graphene being too large in size, unevenly dispersed, and poor heat dissipation effect of the coating.
[0032] The present invention utilizes the high thermal conductivity of the nanographene of the present invention to solve the problem of slow heat dissipation of the existing motor controller, and has an obvious heat dissipation effect, providing strong evidence for subsequent market development.
[0033] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, wherein like reference numerals generally represent like components throughout the exemplary embodiments of the present invention.
[0035] Figure 1 The SEM image of the nanographene provided in Example 1 of the present invention is shown.
[0036] Figure 2 The Raman spectrum (“Counts”, “Ramanshift”) of the nanographene provided in Example 1 of the present invention is shown.
[0037] Figure 3 An AFM (atomic force microscope) image of the nanographene provided in Example 1 of the present invention is shown (AFM is strong evidence for characterizing that a material is nanometer in size and thickness. This image is directly captured from an AFM device. The HeightSensor in the image represents a height sensor. A large number of irregularly shaped flakes can be seen in the image. The surface of the flakes is relatively flat. By measuring their thickness, it is analyzed that the thickness is approximately between 1.5 and 2 nm). DETAILED DESCRIPTION
[0038] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.
[0039] In the following embodiments and comparative examples:
[0040] Expanded graphite micro-flakes were purchased from Qingdao Coastal Carbon Material Technology Co., Ltd., model SYH-5;
[0041] The polyurethane prepolymer used was from Beijing Oriental Yuhong Waterproof Material Co., Ltd., model SPU-311A;
[0042] The second dispersant was purchased from Fujian Langpu New Material Technology Co., Ltd., model S-527;
[0043] The defoamer was purchased from Valin Coatings Co., Ltd., model BYK-065;
[0044] The thixotropic agent was purchased from Zhejiang Hongyu New Materials Co., Ltd., model HY-708;
[0045] The stannous octoate catalyst was purchased from Evonik Specialty Chemicals (Shanghai) Co., Ltd., model T-9;
[0046] Oxazolidine latent curing agent was purchased from Zhejiang Jinfeng New Material Technology Co., Ltd., model JH-366;
[0047] The motor controller is an 18-tube 1000W motor controller from Science Fiction.
[0048] Example 1
[0049] This embodiment provides a method for preparing nanographene, the preparation method comprising the following steps:
[0050] S1: 3 parts of expanded graphite microsheets, 96 parts of deionized water and 1 part of PVP are added into a high-speed disperser and stirred at 1000 r / min to obtain a first mixed material; the first mixed material is processed 3 times by a high-pressure homogenizer at 25 MPa and a feed rate of 0.5 L / s to peel off the expanded graphite microsheets in the first mixed material to obtain a slurry.
[0051] S2: The above mixture is pumped into a sand mill and processed at 1500r / min for 1 hour. The particle size of the solid material obtained by sand milling is reduced to D50 below 5 microns. The material obtained by sand milling is pumped into a plate and frame filter press to obtain a filter cake with a solid content of 16%, which provides an accurate solid content ratio for subsequent high-pressure micro jetting to achieve the best particle size effect.
[0052] S3: Weigh 1 kg of filter cake with a solid content of 16%, 4 kg of deionized water and 20 g of BYK2012 dispersant, add them into a high-speed disperser and stir them evenly at 1000 r / min to obtain a second mixed material; perform high-pressure microfluidization treatment on the second mixed material for 10 times, with a working pressure of 150 MPa, a flow rate of 150 L / h, and a working temperature of 65°C to obtain a dispersion with a solid content of 3.2% nano-graphene.
[0053] Example 2
[0054] This embodiment provides a method for preparing nano-graphene. The difference between this embodiment and embodiment 1 is that:
[0055] The amount of deionized water in step S3 is 3 kg, and a dispersion liquid with a solid content of 4% nanographene is obtained.
[0056] Example 3
[0057] This embodiment provides a method for preparing nano-graphene. The difference between this embodiment and embodiment 1 is that:
[0058] The amount of deionized water in step S3 is 5 kg, and a dispersion liquid with a solid content of 2.6% nanographene is obtained.
[0059] The particle size of the nano-graphene in the nano-graphene dispersion of the above-mentioned Examples 1-3 was tested using a Dandong Better laser particle size analyzer. The results are shown in Table 1.
[0060] Table 1
[0061] D10 / μm D25 / μm D50 / μm D75 / μm D90 / μm Example 1 0.489 0.572 0.743 1.119 1.43 Example 2 0.889 1.275 1.581 1.852 2.14 Example 3 0.291 0.442 0.611 0.745 1.022
[0062] Example 4
[0063] This embodiment provides a nano-graphene polyurethane coating, which includes the following components in parts by weight: 61 parts of polyurethane prepolymer, 9 parts of auxiliary agent and 30 parts of the nano-graphene dispersion described in Example 1.
[0064] The auxiliary agent comprises the following components: a second dispersant, a defoamer, a thixotropic agent, a stannous octoate catalyst and an oxazolidine latent curing agent; the second dispersant, the defoamer, the thixotropic agent and the stannous octoate catalyst are 4 parts in total, and the oxazolidine latent curing agent is 5 parts.
[0065] The preparation method of the nano-graphene polyurethane coating comprises: adding the polyurethane prepolymer, the auxiliary agent and the nano-graphene into a vacuum planetary mixer, stirring at 1000 r / min for 1 hour at (60±2)°C and maintaining a negative pressure of -0.095 MPa, filtering to obtain the nano-graphene polyurethane coating.
[0066] Example 5
[0067] This embodiment provides a nano-graphene polyurethane coating. The only difference between this embodiment and embodiment 4 is: 71 parts of polyurethane prepolymer, 9 parts of auxiliary agent and 20 parts of the nano-graphene dispersion described in embodiment 1.
[0068] Example 6
[0069] This embodiment provides a nano-graphene polyurethane coating. The only difference between this embodiment and embodiment 4 is: 51 parts of polyurethane prepolymer, 9 parts of auxiliary agent and 40 parts of the nano-graphene dispersion described in embodiment 1.
[0070] The present invention uses a NETZSCH laser thermal conductivity meter to measure the thermal conductivity of the coating formed by the nanographene polyurethane coating obtained in Example 4, and the results are shown in Table 2.
[0071] Table 2
[0072]
[0073]
[0074] The thermal conductivity of Examples 5 and 6 is lower than that of Example 4. The main reason is that the proportion of nanographene in Example 5 is lower than that in Example 4, and too little thermal conductive filler causes poor thermal conductivity. The proportion of nanographene in Example 6 is the highest, but the nanographene is added in the form of a dispersion, which causes the coating to be too thin (calculated based on 50% solid content of polyurethane and 3.2% solid content of graphene dispersion, the solid content of Example 4 is 40.46%, and the solid content of Example 6 is 35.78%, so the viscosity of the coating in Example 6 is relatively thin), which makes it easy to sag during spraying, and the spraying effect is poor, resulting in weakened performance. Therefore, Example 4 was selected as the best ratio for subsequent experiments.
[0075] The nano-graphene polyurethane coating obtained in Example 4 is used as a heat dissipation coating for a motor controller, specifically:
[0076] Spray the nanographene polyurethane coating obtained in Example 4 on the motor controller. Spraying is carried out with a manual spray gun. The material must be discharged evenly and atomized well before spraying. The nozzle is about 200mm away from the substrate and is swept evenly from left to right. Ensure that the coating achieves good coverage on the substrate. The wet film thickness is about 60um and the dry film thickness is about 10um. After spraying, it should be left to stand for one minute before baking to achieve better coating flatness and prevent blistering. Curing method: Bake at 120℃ for 15 minutes.
[0077] In order to test the actual heat dissipation effect of the nano-graphene polyurethane coating of Example 4 of the present invention, an 18-tube 1000W motor controller of Science Fiction Company was selected for spraying, and the manufacturer conducted actual testing on electric vehicles.
[0078] For comparison, A-blank sample without heat dissipation coating was selected, and B-oily graphene sample with oily epoxy graphene (micrometer) heat dissipation coating of Suzhou Di Chuang Company was sprayed for comparison. The nanographene polyurethane coating of Example 4 of the present invention is recorded as C-nanographene.
[0079] The experimental parameters are: ambient temperature 5℃, MOS tube (SKD502T), power supply 60V, current 38.5A, external load 800.
[0080] The quality of the heat dissipation coating can be judged by the length of time it takes for the motor controller cavity to reach 80°C after the load is applied. Table 3 shows that:
[0081] Table 3
[0082] Experimental Project A-Blank B-Oily Graphene C-Nanographene Time to heat up to 80 degrees 60min 75min 165min
[0083] The motor controller of the A-blank sample reached the temperature limit in 60 minutes; the motor controller sprayed with B-oily graphene reached the temperature limit in 75 minutes, and the motor controller sprayed with C-nanographene reached the temperature limit in 165 minutes, that is, the heat dissipation performance of the nanographene polyurethane coating of the present invention is more than doubled.
[0084] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A method for preparing nanographene, characterized in that: The preparation method comprises the following steps: S1: Mixing and stirring expanded graphite microsheets, water and an organic solvent to obtain a first mixed material; high-pressure homogenization treatment of the first mixed material to peel off the expanded graphite microsheets in the first mixed material to obtain a liquid slurry; S2: sand-milling and filter-pressing the mixture to obtain a filter cake; S3: mixing the filter cake with water and the first dispersant and stirring them uniformly to obtain a second mixed material; and subjecting the second mixed material to a high-pressure microfluidization treatment to obtain a dispersion of the nano-graphene.
2. The method for preparing nanographene according to claim 1, wherein: In step S1: The organic solvent is at least one of N-methylpyrrolidone, DMF, ethanol and water; The speed of mixing and stirring is 950-1050r / min; The first mixed material is treated with high pressure homogenization for 1-5 times; the working pressure of the high pressure homogenization is 20-30 MPa, and the feed rate is 0.1-1 L / s.
3. The method for preparing nano-graphene according to claim 1, wherein: In step S2: The equipment used for the sand milling process includes a sand mill; the rotation speed of the sand mill is 1400-1600r / min; the sand milling process lasts for 0.8-1.2h; the particle size of the solid material obtained by the sand milling process is D50 less than 5 microns; The solid content of the filter cake is 14-18%.
4. The method for preparing nano-graphene according to claim 1, wherein: In step S3: The mass ratio of the filter cake, water and the first dispersant is (900-1100):(2500-5500):(15-25); The speed of mixing and stirring is 950-1050r / min; The second mixed material is treated with high-pressure microfluidization for 8-12 times; the working pressure of the high-pressure microfluidization treatment is 120-150 MPa, the flow rate is 100-200 L / h, and the working temperature is 60-70°C. The solid content of the nano-graphene dispersion is 2-4.5%.
5. A dispersion of nano-graphene prepared by the method for preparing nano-graphene according to any one of claims 1 to 4.
6. A nanographene polyurethane coating, characterized in that: The coating comprises the following components: a polyurethane prepolymer, an auxiliary agent and the dispersion of the nanographene according to claim 5.
7. The nano-graphene polyurethane coating according to claim 6, wherein: The coating comprises the following components in parts by weight: 15-75 parts of polyurethane prepolymer, 8-10 parts of auxiliary agent and 5-45 parts of nanographene dispersion; The auxiliary agent includes the following components: a second dispersant, a defoamer, a thixotropic agent, a stannous octoate catalyst and an oxazolidine latent curing agent; the ratio of the total mass of the second dispersant, the defoamer, the thixotropic agent and the stannous octoate catalyst to the total mass of the oxazolidine latent curing agent is (3.5-4.5): (4.5-5.5).
8. The method for preparing the nano-graphene polyurethane coating according to claim 6 or 7, characterized in that: The preparation method comprises: mixing the polyurethane prepolymer, the auxiliary agent and the dispersion of nano-graphene, stirring evenly under negative pressure, and filtering to obtain the nano-graphene polyurethane coating.
9. The method for preparing nano-graphene polyurethane coating according to claim 8, wherein: The temperature of the negative pressure stirring is 55-65°C, the pressure of the negative pressure stirring is -0.100 to -0.090MPa, and the rotation speed of the negative pressure stirring is 950-1050r / min.
10. Application of the nano-graphene polyurethane coating according to claim 6 or 7 as a heat dissipation coating for a motor controller.
Citation Information
Patent Citations
Method and device for continuously producing graphene on large scale and graphene prepared through method
CN108622888A
Method for preparing graphene through full liquid water phase physical stripping
CN109052380A
Graphene and preparation method and application thereof
CN109095462A
Preparation methods of high-concentration graphene water-based dispersion liquid and self-dispersion graphene powder
CN110330012A
Graphene heat dissipation coating and preparation method thereof
CN111534177A