Method for auxiliary regeneration of graphite molten salt recovered from battery negative electrode and application of graphite molten salt recovered from battery negative electrode

Through the molten salt-assisted regeneration method, inorganic salt and low-temperature calcination technology, the problems of resource waste and environmental pollution in waste graphite recycling are solved, and efficient purification of graphite and electrochemical performance are achieved, which is suitable for the regeneration of negative electrode materials of lithium-ion batteries. use.

CN118929655AActive Publication Date: 2024-11-12HUNAN LINTE TECH CO LTD +1

Patent Information

Application Number
CN202410991044.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The existing technology is difficult to efficiently recycle and reuse waste graphite, resulting in waste of resources and environmental pollution. Traditional methods require high-temperature calcination and acid treatment, which increases costs and pollution.

Method used

Using molten salt-assisted regeneration method, the impurity content in graphite is significantly reduced by mixing with inorganic salts and low-temperature calcining in the air atmosphere, and the electrochemical performance is improved through water washing, and the high solubility and atomic mixing of low-melting salts are utilized. process, simplify the process and reduce the temperature.

Benefits of technology

It realizes efficient purification and regeneration of graphite, reduces the calcination temperature, improves the reversible capacity and cycle life of graphite, and has a simple process, environmental protection, and low cost, which is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929655A_ABST
    Figure CN118929655A_ABST
Patent Text Reader

Abstract

The invention provides a battery negative electrode graphite molten salt recovery auxiliary regeneration method and application, and the method comprises the following steps: grinding graphite powder recovered from a waste battery negative electrode and inorganic salt, and fully mixing to obtain mixed powder; the mixed powder is calcined in the air atmosphere at the temperature of 800-1100 DEG C; the calcined product is washed, filtered and dried for many times to obtain regenerated graphite, and the regenerated graphite is assisted by simple molten salt and washed with water, so that the impurities in the waste graphite negative electrode material can be obviously reduced, and the electrochemical performance can be obviously improved. The graphite regeneration method disclosed by the invention is simple and easy to implement, and the fused salt can be repeatedly used, so that resource reutilization of the retired lithium ion negative electrode material is promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of waste graphite recovery technology and resource utilization, and in particular to a method and application of battery negative electrode recovery of graphite molten salt assisted regeneration. Background Art

[0002] Graphite is widely used in negative electrode materials of lithium-ion batteries due to its advantages such as good conductivity, high reversible capacity and good cycle stability. As the most commonly used negative electrode material, graphite accounts for 12% to 21% of the total battery weight and is widely used in commercial lithium batteries, especially in the field of power batteries. The booming lithium battery industry has brought a huge number of scrapped batteries, and it is estimated that by 2030, a total of 11 million tons of scrapped lithium batteries will be generated. At present, the recycling technology of retired power batteries focuses on the recycling of positive electrode materials, but the disassembled waste graphite is difficult to achieve efficient utilization due to the lack of effective technical means. Most companies are still at the stage of inefficient incineration as fuel or landfill treatment, resulting in a large waste of resources and environmental pollution.

[0003] The existing conventional waste graphite repair and regeneration technology generally first removes the surface adhesive by high-temperature calcination in an inert atmosphere, then uses acid solution to remove the internal metal impurities, and then obtains the preliminary purified graphite through a series of operations such as drying, ball milling, and screening. The material processing method is relatively cumbersome, and it requires the use of inert atmosphere high-temperature calcination, which greatly increases the processing cost of the enterprise. It also involves the acid treatment process to remove impurities such as metal ions contained in the graphite, which will significantly increase the cost of graphite recovery and regeneration and cause environmental pollution to a certain extent. Therefore, there is an urgent need for a simple, economical, green and environmentally friendly graphite recovery and regeneration technology to obtain purified and regenerated graphite, which is of great significance for the reuse of waste graphite resources in lithium-ion battery negative electrode materials. Summary of the invention

[0004] The present invention provides a method and application for recycling graphite molten salt assisted regeneration of battery negative electrode, the purpose of which is to solve the above-mentioned problems existing in the background technology.

[0005] In order to achieve the above-mentioned purpose, the embodiments of the present invention provide a method and application of graphite molten salt assisted regeneration of battery negative electrode, which can significantly reduce the impurities in the waste graphite negative electrode material and significantly improve the electrochemical performance with the help of simple molten salt assistance and water washing. The graphite regeneration method of the present invention is simple and easy to implement, and the molten salt can be reused, which is conducive to promoting the resource reuse of retired lithium-ion negative electrode materials.

[0006] A method for recycling graphite molten salt assisted regeneration of a battery negative electrode comprises the following steps:

[0007] S1: Grind and fully mix the graphite powder recovered from the negative electrode of the waste battery and the inorganic salt to obtain a mixed powder;

[0008] S2: calcining the mixed powder in an air atmosphere at 800-1100° C.;

[0009] S3: Wash the calcined product several times, filter and dry it to obtain regenerated graphite.

[0010] According to one aspect of an embodiment of the present invention, in step S1, the inorganic salt is sodium chloride.

[0011] According to one aspect of an embodiment of the present invention, in step S1, the mass ratio of graphite powder to inorganic salt is 1:9 to 9:1.

[0012] According to one aspect of an embodiment of the present invention, in step S1, the mass ratio of graphite powder to inorganic salt is 1:1 to 4. Preferably, the mass ratio of graphite powder to inorganic salt includes 1:1, 1:2, 1:3, 1:4.

[0013] According to one aspect of an embodiment of the present invention, in step S2, the calcination time is 0.2 to 4 hours, and the heating rate is 2 to 10°C / min.

[0014] According to one aspect of the embodiment of the present invention, in step S2, the calcination time is 1 hour.

[0015] According to one aspect of the embodiment of the present invention, in step S3, the washing process uses deionized water for immersion and stirring, the water temperature is 25 to 90° C., and the number of washing times is 1 to 3 times.

[0016] Based on an overall concept of the invention, an embodiment of the present invention provides regenerated graphite prepared by the above-mentioned method for recycling graphite from battery negative electrodes with molten salt assistance.

[0017] An embodiment of the present invention also provides the use of the regenerated graphite prepared by the above-mentioned method for recycling graphite from a negative electrode of a battery by molten salt-assisted regeneration in a lithium-ion battery.

[0018] According to one aspect of an embodiment of the present invention, the regenerated graphite is mixed with PVDF and conductive carbon black to form a uniform slurry, which is then coated on a conductive copper foil and dried to obtain a negative electrode for a lithium-ion battery.

[0019] The molten salt calcination method uses one or several low-melting-point salts as calcination media. Since the low-melting-point salts are used as reaction media, a liquid phase appears during the synthesis process, which increases the solubility of the reactants in the molten salt medium, greatly accelerates the diffusion rate of ions, and enables the calcination reactants to achieve atomic-scale mixing in the liquid phase. The calcination reaction can be carried out at the atomic level, and the calcination reaction process is highly efficient. After the reaction is completed, the salts are dissolved in a suitable solvent, and the calcined product can be obtained after filtering and washing. Compared with conventional high-temperature calcination methods, this method has the advantages of simple process, low synthesis temperature, short insulation time, and high processing efficiency. Therefore, the molten salt calcination method utilizes its advantages of low calcination temperature, high solubility, atomic-level mixing process, and easy separation and recycling of salts. It is expected to reduce the calcination temperature in the molten salt-assisted process of graphite recovery, and remove impurities in graphite by utilizing the high solubility and atomic-level mixing process of molten salt, thereby developing a new type of graphite recovery purification and reuse technology.

[0020] The molten salt assisted regeneration technology of the present invention has the following effects:

[0021] A. In the field of traditional waste graphite recycling and reuse, since graphite contains impurities such as binders and electrolytes, it is necessary to perform high-temperature calcination on the graphite to remove organic impurities. However, the traditional process of calcination using an inert atmosphere will leave a small amount of organic matter remaining to form amorphous carbon, affecting the electrochemical properties of graphite. This application cleverly uses molten salt to assist the low-temperature calcination process in an air atmosphere to completely oxidize and remove organic carbon before the molten salt melts. After the molten salt melts, a liquid phase is formed to protect the graphite from further oxidation, resulting in burnout losses.

[0022] B. Calcination in an air atmosphere in a muffle furnace. Before the low-melting-point molten salt melts, the graphite will undergo surface oxidation. The oxygen in the air reacts with the graphite at the gas-solid interface, reducing the active points on the graphite surface and reducing the first irreversible capacity loss. At the same time, more micropores and nanopores are generated to increase the storage space for lithium ions, which is beneficial to improving the reversible capacity and the negative electrode performance. In addition, the oxide layer formed during oxidation is tightly combined with the graphite to form a dense passivation film, which prevents the electrolyte from solvating the graphite and improves the reversible capacity of the graphite.

[0023] C. Inorganic salts have an extraordinary solubility for reactants in a molten state, low viscosity, and fast diffusion. They can drive the impurity ions in graphite to migrate from the deep layer of graphite to the surface through concentration difference. After cooling, they can be removed by washing with water, which greatly reduces the negative impact of inorganic impurities such as Ni, Co, and Mn in waste graphite on the lithium storage capacity and cycle life of graphite negative electrodes. Compared with other cleaning methods such as pickling, it has the advantages of being green, simple to operate, low cost, and easy to scale production.

[0024] The above scheme of the present invention has the following beneficial effects:

[0025] (1) The present invention provides a method for recycling graphite from a battery negative electrode by molten salt-assisted regeneration. With the aid of simple molten salt and water washing, the impurities in the waste graphite negative electrode material can be significantly reduced, and the electrochemical performance can be significantly improved. The graphite regeneration method is simple and easy to implement, and the molten salt can be reused, which is conducive to promoting the resource reuse of retired lithium-ion negative electrode materials.

[0026] (2) The present invention provides a method for regenerating waste graphite using molten salt. The prepared regenerated graphite negative electrode material, when used as a negative electrode material for lithium-ion batteries, has better electrochemical properties than the regenerated graphite material prepared by conventional high-temperature heat treatment and acid washing and impurity removal processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 It is a schematic flow chart of a method for recovering graphite molten salt assisted regeneration of a battery negative electrode according to Example 1 of the present invention;

[0029] Figure 2 The SEM images of the samples of the recycled graphite waste (a), Comparative Example 1 (b), Comparative Example 2 (c), and Example 1 (d) of the present invention are shown;

[0030] Figure 3 This is a schematic diagram of the cycle stability of a negative electrode assembled with regenerated graphite at a 0.1C rate performance, prepared by a method for recycling graphite molten salt assisted regeneration of a battery negative electrode according to Example 1 of the present invention. DETAILED DESCRIPTION

[0031] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0032] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0033] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0034] In view of the existing problems, the present invention provides a method for recycling graphite molten salt assisted regeneration of battery negative electrode, the process is as follows Figure 1 As shown, the following steps are included:

[0035] S1: Grind and fully mix the graphite powder recovered from the negative electrode of the waste battery and the inorganic salt to obtain a mixed powder;

[0036] S2: calcining the mixed powder in an air atmosphere at 800-1100° C.;

[0037] S3: Wash the calcined product several times, filter and dry it to obtain regenerated graphite.

[0038] According to one aspect of an embodiment of the present invention, in step S1, the inorganic salt is sodium chloride.

[0039] According to one aspect of an embodiment of the present invention, in step S1, the mass ratio of graphite powder to inorganic salt is 1:9 to 9:1.

[0040] According to one aspect of an embodiment of the present invention, in step S1, the mass ratio of graphite powder to inorganic salt is 1:1 to 4. Preferably, the mass ratio of graphite powder to inorganic salt includes 1:1, 1:2, 1:3, 1:4.

[0041] According to one aspect of an embodiment of the present invention, in step S2, the calcination time is 0.2 to 4 hours, and the heating rate is 2 to 10°C / min.

[0042] According to one aspect of the embodiment of the present invention, in step S2, the calcination time is 1 hour.

[0043] According to one aspect of the embodiment of the present invention, in step S3, the washing process uses deionized water for immersion and stirring, the water temperature is 25 to 90° C., and the number of washing times is 1 to 3 times.

[0044] Based on an overall concept of the invention, an embodiment of the present invention provides regenerated graphite prepared by the above-mentioned method for recycling graphite from battery negative electrodes with molten salt assistance.

[0045] An embodiment of the present invention also provides the use of the regenerated graphite prepared by the above-mentioned method for recycling graphite from a negative electrode of a battery by molten salt-assisted regeneration in a lithium-ion battery.

[0046] According to one aspect of an embodiment of the present invention, the regenerated graphite is mixed with PVDF and conductive carbon black to obtain a mixture which is dispersed in an N-methylpyrrolidone (NMP) solution to form a uniform slurry, which is then coated on a conductive copper foil and dried to obtain a negative electrode for a lithium-ion battery.

[0047] The following is a detailed description through specific embodiments.

[0048] Example 1

[0049] A method for recycling graphite molten salt assisted regeneration of a battery negative electrode comprises the following steps:

[0050] S1. Grind 2 g of recycled graphite waste and 2 g of sodium chloride for 10 min to fully mix to obtain a mixed powder;

[0051] S2. The mixed powder was directly placed in a muffle furnace in an air atmosphere and calcined at 850°C for 1 h at a heating rate of 10°C / min;

[0052] S3. The calcined product was washed with 80° C. deionized water for 3 times, each washing time was 2 h, and the regenerated graphite was obtained after filtering and drying.

[0053] The above-mentioned regenerated graphite is used as a negative electrode material for assembling a lithium-ion battery, comprising the following steps:

[0054] A1: The above-mentioned regenerated graphite, PVDF and conductive carbon black are mixed uniformly in a mass ratio of 8:1:1, dispersed in an NMP solution to form a uniform slurry, and then the slurry is coated on a copper foil and vacuum dried at 120° C. to obtain a graphite electrode sheet.

[0055] A2: Pair the graphite electrode sheet with the metal lithium negative electrode, assemble a CR2016 button cell in the inert atmosphere of the glove box, and test the electrochemical performance of the hard carbon electrode. The button cell structure includes a positive electrode shell (stainless steel), a negative electrode shell (stainless steel), a gasket (stainless steel), a hard carbon electrode, a lithium sheet, an electrolyte, and a separator (PP).

[0056] Example 2

[0057] A method for recovering graphite molten salt assisted regeneration of a battery negative electrode (calcination time is different from that in Example 1), comprising the following steps:

[0058] S1. Grind 2 g of recycled graphite waste and 2 g of sodium chloride for 10 min to fully mix to obtain a mixed powder;

[0059] S2. The mixed powder was directly placed in a muffle furnace in an air atmosphere and calcined at 850°C for 0.5 h at a heating rate of 10°C / min;

[0060] S3. The calcined product was washed with 80° C. deionized water for 3 times, each washing time was 2 h, and the regenerated graphite was obtained after filtering and drying.

[0061] Example 3

[0062] The difference is that the mass ratio of the recycled graphite waste and sodium chloride is 1:2, and the other steps are the same as in Example 1.

[0063] Example 4

[0064] The difference is that the mass ratio of the recycled graphite waste and sodium chloride is 1:3, and the other steps are the same as in Example 1.

[0065] Comparative Example 1

[0066] Compared with the treatment method of Example 1, Comparative Example 1 does not add inorganic salt during the calcination process, and includes the following steps:

[0067] S1, grind 2g of recycled graphite waste for 10min;

[0068] S2. The ground graphite waste is placed in a muffle furnace filled with air and calcined at 850°C for 1 hour at a heating rate of 10°C / min to obtain.

[0069] Comparative Example 2

[0070] Compared with the treatment method of Example 1, this comparative example is a conventional high-temperature calcination and pickling process, comprising the following steps:

[0071] S1. 2 g of recycled graphite waste was placed in a tube furnace in an argon atmosphere and calcined at 850 °C for 1 h at a heating rate of 10 °C / min;

[0072] S2. Wash the calcined product with 1 mol / L sulfuric acid and deionized water respectively, filter and dry to obtain regenerated graphite.

[0073] Comparative Example 3

[0074] A method for recovering graphite molten salt assisted regeneration of a battery negative electrode (the type of inorganic salt is different from that in Example 1), comprising the following steps:

[0075] S1. Grind 2 g of recycled graphite waste and 2 g of potassium chloride for 10 min to fully mix to obtain a mixed powder;

[0076] S2. The mixed powder was directly placed in a muffle furnace in an air atmosphere and calcined at 850°C for 1 h at a heating rate of 10°C / min;

[0077] S3. The calcined product was washed with 80° C. deionized water for 3 times, each washing time was 2 h, and the regenerated graphite was obtained after filtering and drying.

[0078] Comparative Example 4

[0079] The difference is that the type of inorganic salt is sodium nitrate, and the other steps are the same as Example 1.

[0080] Comparative Example 5

[0081] The difference is that the type of inorganic salt is sodium carbonate, and the other steps are the same as Example 1.

[0082] Comparative Example 6

[0083] The difference is that the type of inorganic salt is sodium sulfate, and the other steps are the same as Example 1.

[0084] Comparative Example 7

[0085] A method for recovering graphite molten salt assisted regeneration of a battery negative electrode (the type of inorganic salt is different from that in Example 1), comprising the following steps:

[0086] S1. Grind 2 g of recycled graphite waste and 2 g of a mixed molten salt of sodium chloride and sodium sulfate (mass ratio of the mixed molten salt is 1:1) for 10 min to fully mix to obtain a mixed powder;

[0087] S2. The mixed powder was directly placed in a muffle furnace in an air atmosphere and calcined at 850°C for 1 h at a heating rate of 10°C / min;

[0088] S3. Water washing and purification: The calcined product was washed with 80° C. deionized water for 3 times, each washing time was 2 h, and the regenerated graphite was obtained after filtration and drying.

[0089] Comparative Example 8:

[0090] A method for recovering graphite molten salt assisted regeneration of a battery negative electrode (calcination temperature is different from that in Example 1), comprising the following steps:

[0091] S1. Grind 2 g of recycled graphite waste and 2 g of sodium chloride for 10 min to fully mix to obtain a mixed powder;

[0092] S2. The mixed powder was directly placed in a muffle furnace in an air atmosphere and calcined at 750°C for 1 h at a heating rate of 10°C / min;

[0093] S3. The calcined product was washed with 80° C. deionized water for 3 times, each washing time was 2 h, and the regenerated graphite was obtained after filtering and drying.

[0094] Characterization and performance testing

[0095] like Figure 2 The following are SEM photos of the samples of the recycled graphite waste (a), Comparative Example 1 (b), Comparative Example 2 (c), and Example 1 (d) of the present invention. Figure 2 It can be seen that there are a lot of attachments on the surface of the graphite sheets of recycled graphite waste. After the muffle furnace is burned in the air, the attachments on the surface of the graphite sheets can be removed by oxidation process to obtain graphite particles with a relatively smooth surface. However, it is difficult to remove impurities on the surface of the graphite sheets by calcining in an inert atmosphere. Molten salt-assisted muffle furnace burning can also obtain graphite particles with a relatively smooth surface.

[0096] Taking the button batteries assembled with recycled graphite prepared in Examples 1 to 4 and Comparative Examples 1 to 8 as examples, the battery performances of the batteries assembled with recycled graphite electrodes prepared in Examples 1 to 4 and Comparative Examples 1 to 8 were evaluated using a charging and discharging device (Blue Electric 3001). The results are shown in Table 1.

[0097] Table 1 The charge and discharge capacity and initial performance of the batteries assembled with the prepared regenerated graphite electrodes of Examples 1 to 4 and Comparative Examples 1 to 8 at a rate of 0.1C

[0098]

[0099]

[0100] The results in Table 1 show that under the first charge and discharge of 0.1C, the first discharge specific capacities of the negative electrodes prepared by sodium chloride molten salt (Example 1), sodium sulfate + sodium chloride molten salt (Comparative Example 7) and potassium chloride molten salt (Comparative Example 3) are 385.70mAh / g, 340.68mAh / g and 323.92mAh / g, respectively, and the charge specific capacities are 295.30mAh / g, 256.42mAh / g and 246.43mAh / g, respectively, and the first coulombic efficiencies are 76.56%, 75.27% and 76.08%, respectively. The technical effect of using sodium chloride molten salt in Example 1 of the present invention is obviously better than that of other molten salts and their combinations. In Comparative Example 1, the regenerated graphite negative electrode prepared by direct empty firing without molten salt treatment (the first discharge / charge specific capacity is 329.62 mAh / g and 249.5 mAh / g, and the first coulombic efficiency is 75.69%), while the regenerated graphite obtained by conventional calcination and acid treatment has a discharge / charge specific capacity of 322.54 mAh / g and 232.10 mAh / g, respectively. In comparison, the molten salt assistance of the present invention can significantly improve the specific capacity of the regenerated graphite.

[0101] In addition, the first discharge specific capacity of the regenerated graphite electrode prepared by sodium chloride molten salt (calcination temperature of comparative example 8 is 750°C) and sodium chloride molten salt (calcination time of example 2 is 0.5h) is 310.54mAh / g and 354.3mAh / g respectively, the charge specific capacity is 229.41mAh / g and 278.65mAh / g respectively, and the first coulomb efficiency is 73.88% and 78.65%. The first charge and discharge specific capacity is lower than that of example 1 (calcination temperature is 850°C and time is 1h). It can be seen that the calcination temperature and time also have a significant effect on the electrochemical properties of the regenerated graphite negative electrode.

[0102] Figure 3The cycle stability test of the negative electrode material in Example 1 of the present invention at 0.1C rate performance shows good stability and capacity retention. The above results show that the method of recycling graphite molten salt assisted regeneration of a battery negative electrode of the present invention significantly improves the electrochemical performance of the regenerated graphite negative electrode material.

[0103] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for recovering graphite molten salt assisted regeneration of battery negative electrode, characterized in that: The steps include: S1: Grind and fully mix the graphite powder recovered from the negative electrode of the waste battery and the inorganic salt to obtain a mixed powder; S2: calcining the mixed powder in an air atmosphere at 800-1100° C.; S3: Wash the calcined product several times, filter and dry it to obtain regenerated graphite.

2. A method for recovering graphite molten salt assisted regeneration according to claim 1, characterized in that: In step S1, the inorganic salt is sodium chloride.

3. The method for recovering graphite molten salt assisted regeneration of a battery negative electrode according to claim 1, characterized in that: In step S1, the mass ratio of graphite powder to inorganic salt is 1:9 to 9:

1.

4. The method for recovering graphite molten salt assisted regeneration of a battery negative electrode according to claim 1, characterized in that: In step S1, the mass ratio of graphite powder to inorganic salt is 1:1-4.

5. The method for recovering graphite molten salt assisted regeneration of a battery negative electrode according to claim 1, characterized in that: In step S2, the calcination time is 0.2 to 4 hours, and the heating rate is 2 to 10°C / min.

6. The method for recovering graphite molten salt assisted regeneration of a battery negative electrode according to claim 1, characterized in that: In step S2, the calcination time is 1 hour.

7. The method for recovering graphite molten salt assisted regeneration of a battery negative electrode according to claim 1, characterized in that: In step S3, the washing process uses deionized water for immersion and stirring, the water temperature is 25 to 90° C., and the washing times are 1 to 3 times.

8. Regenerated graphite prepared by the method for molten salt-assisted regeneration of graphite for battery negative electrode recovery as described in any one of claims 1 to 7.

9. Use of the regenerated graphite prepared by the method for recycling graphite from a battery negative electrode by molten salt-assisted regeneration as described in any one of claims 1 to 7 in lithium-ion batteries.

10. The use according to claim 9, characterized in that: The regenerated graphite is mixed with PVDF and conductive carbon black to obtain a mixture which is dispersed in an N-methylpyrrolidone solution to form a uniform slurry, and then the slurry is coated on a conductive copper foil and dried to obtain a negative electrode of a lithium ion battery.

Citation Information

Patent Citations

  • Graphite lithium ion battery negative electrode material with multiple layers of graphene surfaces and preparation method thereof

    CN108134085A

  • Recovery method of waste lithium ion battery negative electrode material

    CN111430831A

  • Method for preparing high-purity porous graphite

    CN114477160A

  • Powder comprising carbon nanostructures and its method of production

    US20150056513A1

Cited By

  • Battery negative electrode high-valued regeneration system based on multi-source solid waste

    CN119972745A

  • A high-value battery negative electrode regeneration system based on multi-source solid waste

    CN119972745B