Impurity removal method for heavy metal arsenic in graphite powder
Through the synergistic effect of the mixed solution of ferrous sulfate and hydroxylamine and EDTA, the pH value and reduction properties are adjusted, and the problem of wastewater and waste residue treatment when heavy metal arsenic is removed in graphite powder is solved, and high-efficiency arsenic under low iron and low complexing agent conditions are achieved. Removal improves the purity and environmental protection of graphite powder.
Patent Information
- Application Number
- CN202411147978.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When removing heavy metal arsenic from graphite powder, the prior art has problems in the treatment of wastewater and waste slag, and the iron sludge yield is large and the amount of complexing agent is added too large, resulting in pollution and treatment difficulties.
Use a mixed aqueous solution of ferrous sulfate and hydroxylamine to react with complexing agent (such as EDTA) to adjust the pH value to 7-9, adsorb arsenic by forming iron hydroxide, and use the reducing properties of hydroxylamine to reduce the oxidation state of iron and reduce the The amount of iron and complexing agent used to achieve arsenic removal under low iron and low complexing agent conditions.
Effectively remove heavy metal arsenic from graphite powder, reduce the generation of wastewater and waste residue, reduce the use of iron and complexing agents, and improve removal efficiency and environmental protection.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-purity graphite powder purification technology, and in particular to a method for removing impurities of heavy metal arsenic in graphite powder. Background Art
[0002] Graphite is a high-energy crystalline carbon material. Due to its structure and electrical conductivity, thermal conductivity, lubricity, high temperature resistance, and stable chemical properties, it has a high use value among high-performance materials and is widely used in metallurgy, machinery, environmental protection, chemical industry, refractory, electronics, medicine, military industry, aerospace and other fields. Graphite is a very good energy-saving and environmentally friendly material. With the development of modern science and technology and industry, the application field of graphite is constantly expanding. It has become an important raw material for new composite materials in the high-tech field and plays an important role in the national economy. With the continuous development of new technologies and new processes, ordinary high-purity graphite materials can no longer meet the needs of many industries. The quality of graphite purification determines the use characteristics and comprehensive performance of graphite materials. The higher the purity of graphite, the higher the application value.
[0003] The main heavy metal impurities in natural graphite include lead, arsenic, mercury, cadmium, etc., among which arsenic is mainly trivalent arsenic and pentavalent arsenic; there are various forms of arsenic in natural graphite, and various forms of arsenic are difficult to separate from graphite.
[0004] The lime-iron salt method mainly generates a precipitate through the reaction of lime (calcium hydroxide) and iron salt (such as ferrous sulfate), thereby converting arsenate into a precipitate that is insoluble in water to remove arsenic. However, the problem is that a large amount of wastewater and waste residue will be generated after the reaction, which is difficult to handle in the subsequent steps.
[0005] The use of ferrous sulfate and complexing agents to treat heavy metals has technical bottlenecks such as a narrow pH response range, a large amount of ferrous sulfate added, and a high iron sludge output. 2+ -EDTA) as an initiator, the pH response range was significantly expanded, but it also introduced organic secondary pollution and increased the difficulty of removing dissolved iron. Summary of the invention
[0006] In order to solve the above problems, the present invention provides a method for removing heavy metal arsenic from graphite powder, which can effectively remove various forms of heavy metal arsenic in graphite powder, with less wastewater and waste residue generated in the rear, and realize the elimination of metal arsenic under the conditions of low iron dosage and low complexing agent dosage.
[0007] The present invention is achieved in that: A method for removing heavy metal arsenic from graphite powder comprises the following steps: (1) adding a mixed aqueous solution of ferrous sulfate and hydroxylamine to graphite powder, wherein the mass percentage of graphite powder is 10%-20%, adjusting the pH value of the solution to 7-9, wherein the molar mass ratio of ferrous ions to saline hydroxylamine in the mixed aqueous solution of ferrous sulfate and hydroxylamine is (10-30):1, and the molar concentration of ferrous ions in the mixed aqueous solution of ferrous sulfate and hydroxylamine is 0.1-2 mol / L; Add the complexing agent solution to the mixed solution, the molar ratio of ferrous sulfate to complexing agent is 0.8:1-1.5:1, and stir to react for 10-30 minutes; (2) Repeatedly filter and wash until the pH value of the washing liquid is 6.5-7.5; (3) Drying of graphite powder.
[0008] Preferably, the graphite powder is alkali washed, acid washed, and then washed with water for multiple times before the treatment until the washing liquid is 6.5-7.5.
[0009] Preferably, the alkali washing refers to soaking the graphite powder in a NaOH solution with a pH of 12-13, and stirring for 5-15 minutes.
[0010] Preferably, the pickling refers to adding acetic acid solution to the graphite powder, the pH of the acetic acid solution is 4-6, and stirring is maintained for 5-15 minutes.
[0011] Preferably, the complexing agent is any one or more of EDTA or hydrogen peroxide.
[0012] The present invention provides a method for removing heavy metal arsenic from graphite powder, and its beneficial effects include: (1) Ferrous sulfate hydrolyzes in aqueous solution to form iron hydroxides, which adsorb and co-precipitate arsenic by forming iron hydroxides (such as Fe(OH)3). These iron hydroxides have a strong affinity for arsenic and can form insoluble arsenate or arsenite precipitates.
[0013] (2) Hydroxylamine (NH2OH) is a reducing agent that can reduce certain oxidants. 3+ Hydroxylamine exists in the form of NH3OH+ under acidic conditions and has strong reducing properties. Hydroxylamine can be used to reduce Fe in ferrous sulfate. 3+ Converted to Fe 2+ , producing non-toxic gas.
[0014] (3) Adding reducing hydroxylamine (HA) to the Fe2+-EDTA / H2O2 system can inactivate Fe 3+ -EDTA is converted into active Fe 2+ -EDTA, thereby achieving the elimination of organic pollutants under the conditions of low iron dosage and low chelating agent dosage.
[0015] (4) The problem of excessive dosage of reagents and subsequent poor disposal of iron ions in the reaction enhanced by chelating agents was solved. DETAILED DESCRIPTION
[0016] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Specific embodiments
[0017] Weigh 50g of graphite powder, add a salt water hydroxylamine solution of ferrous sulfate to the graphite powder, the molar mass ratio of ferrous ions to salt water hydroxylamine in the mixed aqueous solution of ferrous sulfate and hydroxylamine is 15:1, the molar concentration of ferrous ions in the mixed aqueous solution of ferrous sulfate and hydroxylamine is 1.5mol / L, the mass percentage of graphite powder to salt water hydroxylamine solution of ferrous sulfate is 10%, and acetic acid is used to adjust the pH value of the solution to 7-9. Add an appropriate amount of complexing agent to the mixed solution, the complexing agent in this specific embodiment is EDTA, the molar ratio of ferrous sulfate to complexing agent is 1:1, and the pH value of the solution is adjusted to between 7-9 with salt water or acetic acid, stir appropriately and react for 35 minutes, and then separate the modified natural zeolite from the solution, filter, wash multiple times, and dry. Specific embodiments
[0018] Weigh 50g of graphite powder, wash it with 500ml of sodium hydroxide solution with a pH of 12.2, and stir it for 15 minutes. Filter to get graphite powder, wash the graphite powder repeatedly with pure water, and use pH test paper to detect the washing water to 6.5-7.5.
[0019] Add 500 ml of phosphoric acid solution with a pH of 4.2 to the graphite powder obtained by filtration for acid washing, and stir appropriately for 15 minutes. Filter to obtain graphite powder, wash the graphite powder repeatedly with pure water, and use pH test paper to detect the washing water to 6.5-7.5.
[0020] The washed graphite powder is added with a salt water hydroxylamine solution of ferrous sulfate, wherein the molar mass ratio of ferrous ions to salt water hydroxylamine in the mixed aqueous solution of ferrous sulfate and hydroxylamine is 10:1, the molar concentration of ferrous ions in the mixed aqueous solution of ferrous sulfate and hydroxylamine is 2 mol / L, the mass percentage of graphite powder to salt water hydroxylamine solution of ferrous sulfate is 18%, and acetic acid is used to adjust the pH value of the solution to 7-9. An appropriate amount of complexing agent is added to the mixed solution, and the complexing agent in this specific embodiment is EDTA, and the molar ratio of ferrous sulfate to complexing agent is 1.2:1. The pH value of the solution is adjusted to between 7-9 with salt water or acetic acid, and the solution is stirred and reacted for 30 minutes, and then the modified natural zeolite is separated from the solution, filtered, washed multiple times, and dried. Specific embodiments
[0021] Weigh 50g of graphite powder, wash it with 500ml of sodium hydroxide solution with a pH of 13, and stir it for 5 minutes. Filter to get graphite powder, wash the graphite powder repeatedly with pure water, and use pH test paper to detect the washing water to 6.5-7.5.
[0022] Add 500 ml of phosphoric acid solution with a pH of 6.0 to the graphite powder obtained by filtration for acid washing, and stir appropriately for 5 minutes. Filter to obtain graphite powder, wash the graphite powder repeatedly with pure water, and use pH test paper to detect the washing water to 6.5-7.5.
[0023] The washed graphite powder is added with a salt water hydroxylamine solution of ferrous sulfate, wherein the molar mass ratio of ferrous ions to salt water hydroxylamine in the mixed aqueous solution of ferrous sulfate and hydroxylamine is 30:1, the molar concentration of ferrous ions in the mixed aqueous solution of ferrous sulfate and hydroxylamine is 0.1 mol / L, the mass percentage of graphite powder to salt water hydroxylamine solution of ferrous sulfate is 20%, and acetic acid is used to adjust the pH value of the solution to 7-9. An appropriate amount of complexing agent is added to the mixed solution, and the complexing agent in this specific embodiment is EDTA, and the molar ratio of ferrous sulfate to complexing agent is 1.0:1. The pH value of the solution is adjusted to between 7-9 with salt water or acetic acid, and the solution is stirred and reacted for 20 minutes, and then the modified natural zeolite is separated from the solution, filtered, washed multiple times, and dried. Specific embodiments
[0024] Weigh 50g of graphite powder, wash it with 500ml of sodium hydroxide solution with a pH of 12.5, stir it for 10 minutes, filter it to get graphite powder, wash it repeatedly with pure water, and use pH test paper to check the washing water to 6.5-7.5.
[0025] Add 500 ml of phosphoric acid solution with a pH of 5.0 to the graphite powder obtained by filtration for acid washing, and stir appropriately for 10 minutes. Filter to obtain graphite powder, wash the graphite powder repeatedly with pure water, and use pH test paper to detect the washing water to 6.5-7.5.
[0026] The washed graphite powder is added with a salt water hydroxylamine solution of ferrous sulfate, the molar mass ratio of ferrous ions to salt water hydroxylamine in the mixed aqueous solution of ferrous sulfate and hydroxylamine is 20:1, the molar concentration of ferrous ions in the mixed aqueous solution of ferrous sulfate and hydroxylamine is 1 mol / L, the mass percentage of graphite powder to salt water hydroxylamine solution of ferrous sulfate is 15%, and the pH value of the solution is adjusted to 7-9 with acetic acid. An appropriate amount of complexing agent is added to the mixed solution, and the complexing agent in this specific embodiment is EDTA, and the molar ratio of ferrous sulfate to complexing agent is 0.8:1. The pH value of the solution is adjusted to between 7-9 with salt water or acetic acid, and the solution is stirred and reacted for 40 minutes, and then the modified natural zeolite is separated from the solution, filtered, washed multiple times, and dried.
[0027] In the operation process described in Specific Embodiments 1 to Specific Embodiments 4, the arsenic content in the graphite powder before and after treatment was detected respectively, and the detection method adopted was graphite furnace atomic absorption spectrometry (GFAAS). The detection results were: the arsenic content in the graphite powder before treatment was 0.423-0.578 mg / kg, and the arsenic content of the graphite powder treated by the impurity removal method described in this specific implementation method was 0.0102-0.0357 mg / kg after detection, and the average recovery rate was 95.4%.
Claims
1. A method for removing heavy metal arsenic from graphite powder, characterized in that: The steps are as follows: (1) adding a mixed aqueous solution of ferrous sulfate and hydroxylamine to graphite powder, wherein the mass percentage of graphite powder is 10%-20%, adjusting the pH value of the solution to 7-9, wherein the molar mass ratio of ferrous ions to saline hydroxylamine in the mixed aqueous solution of ferrous sulfate and hydroxylamine is (10-30):1, and the molar concentration of ferrous ions in the mixed aqueous solution of ferrous sulfate and hydroxylamine is 0.1-2 mol / L; (2) Adding a complexing agent solution to the mixed solution, the molar ratio of ferrous sulfate to complexing agent being 0.8:1-1.5:1, and stirring the mixture for 10-30 minutes; (3) Repeatedly filter and wash until the pH value of the washing liquid is 6.5-7.5; (4) Drying of graphite powder.
2. The method for removing heavy metal arsenic from graphite powder according to claim 1, characterized in that: Before treatment, the graphite powder is alkali washed, acid washed, and then washed with water for multiple times until the washing liquid is 6.5-7.
5.
3. The method for removing heavy metal arsenic from graphite powder according to claim 2, characterized in that: The alkaline washing refers to soaking the graphite powder in a NaOH solution with a pH of 12-13 and stirring for 5-15 minutes.
4. The method for removing heavy metal arsenic from graphite powder according to claim 2, characterized in that: The pickling refers to adding acetic acid solution to the graphite powder, the pH of the acetic acid solution is 4-6, and stirring is maintained for 5-15 minutes.
5. The method for removing heavy metal arsenic from graphite powder according to claim 1, characterized in that: The complexing agent is any one or more of EDTA or hydrogen peroxide.
Citation Information
Patent Citations
Hydroxylamine modified polyacrylonitrile-iron complex hydrogen peroxide oxidation arsenic removal method
CN105152303A
Method for treating produced water
CN112441657A
Method for treating arsenic containing solution
JP2008119690A
Process for recovering metal values from materials containing arsenic
US4244734A