Waste photovoltaic graphite-based regenerated graphite negative electrode active material as well as preparation and application thereof

By performing gradient gas change and modification treatment on waste photovoltaic graphite materials, combined with spray granulation and carbonization coating, the electrochemical performance problems of waste photovoltaic graphite materials under high surface load are solved, and its excellent performance in batteries is achieved and fast charging performance.

CN118929657AActive Publication Date: 2024-11-12CENT SOUTH UNIV

Patent Information

Application Number
CN202411165472.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

There is a lack of effective methods in the prior art to recover and regenerate waste photovoltaic graphite materials, especially graphite negative electrode active materials with excellent fast charging performance under high surface loads are difficult to obtain.

Method used

By performing two-stage gradient gas-changing treatment on waste photovoltaic graphite materials, combining spray granulation with modifier and boron-containing modifier, carbonization and carbon coating treatment, it breaks through its physical and chemical characteristics and selectively removes electrochemical harmful impurities. Optimize the structure to suit battery applications.

Benefits of technology

It achieves excellent electrochemical performance and fast charging performance of graphite materials under high surface load, adapts to battery application requirements, and especially improves its liquid absorption performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929657A_ABST
    Figure CN118929657A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of waste photovoltaic graphite material recovery, and particularly relates to a preparation method of a waste photovoltaic graphite-based regenerated graphite negative electrode active material, which comprises the following steps: crushing a graphite block material from a waste photovoltaic source, screening to obtain graphite powder, and then carrying out two-stage gradient variable gas treatment on the graphite powder to obtain pretreated graphite; dispersing the pretreated graphite in water for pulpifying, then adding a modifier with a formula A structure # imgabs0 #, carrying out modification treatment under the assistance of ultrasonic waves, and then carrying out solid-liquid separation and drying to obtain modified graphite; dispersing the modified graphite, a boron-containing modifier and a carbon source through a solvent, and then carrying out spray granulation treatment to obtain particles; and carrying out carbonization treatment on particles obtained by spraying, and then carrying out carbon coating treatment to obtain the waste photovoltaic graphite-based regenerated graphite negative electrode active material. The invention also comprises the active material obtained by the method and application of the active material. The method provided by the invention realizes regeneration of the photovoltaic waste graphite to obtain the active material with high electrochemical performance for the first time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of recycling waste photovoltaic materials, and in particular to the field of regenerating graphite negative electrode active materials from waste photovoltaic graphite materials. Background Art

[0002] With the rise of the photovoltaic industry, the volume of photovoltaic waste is increasing. Photovoltaic waste mainly includes silicon materials, silicon carbide materials and graphite. However, the existing technology mainly involves the recycling of silicon-based materials.

[0003] For example, a Chinese patent document with publication number CN117263189A discloses a method for preparing a silicon-carbon composite material using photovoltaic squared wet silicon powder, the steps of which are: purifying photovoltaic squared wet silicon powder by sulfuric acid roasting to obtain purified silicon powder; purifying waste power battery graphite negative electrode by sulfuric acid and hydrogen peroxide to obtain purified graphite; and high-energy ball milling the purified silicon powder and purified graphite powder to obtain a silicon-carbon composite material.

[0004] For another example, a Chinese patent document with publication number CN104112850A discloses a method for preparing anode materials for lithium-ion batteries based on high-purity silicon waste from the photovoltaic industry. Specifically, a series of treatments are performed on the high-purity silicon waste generated in the process of silicon wafer cutting in the photovoltaic industry, including purification, etching, surface modification, and mixing the treated silicon with graphite negative electrode materials in proportion, to obtain micron or submicron silicon or silicon-graphite mixed materials with controllable structure and composition.

[0005] For another example, a Chinese patent document with publication number CN117096329A discloses a method for preparing a low-cost silicon-graphite negative electrode active material and its application. First, photovoltaic crystalline silicon waste is used as a raw material, a copper alloy additive is added, and an alloying treatment is performed to obtain a porous silicon material. Then asphalt is added and dry ball milling modification is performed. Next, high-temperature carbonization is performed to form a modified porous silicon material coated with amorphous carbon. Then, the modified porous silicon material is dispersed and composited with nanographite to obtain a modified silicon-graphite negative electrode active material in which the modified porous silicon is uniformly doped on flaky graphite.

[0006] In summary, for the recycling of photovoltaic waste, it is still mainly about the recycling and regeneration of silicon-based materials. There are few recycling methods for graphite waste that is widely present in the photovoltaic industry. In particular, the regeneration of graphite negative electrode active materials from waste photovoltaic graphite waste is still a blank in the industry. Summary of the invention

[0007] In order to fill the industry gap in recycled graphite negative electrode active materials from waste photovoltaic graphite materials, the first purpose of the present invention is to provide a method for preparing recycled graphite negative electrode active materials based on waste photovoltaic graphite, aiming to obtain graphite negative electrode active materials with high electrochemical performance based on the regeneration of waste photovoltaic graphite materials.

[0008] The second purpose of the present invention is to provide a waste photovoltaic graphite-based regenerated graphite negative electrode active material prepared by the preparation method and its application in batteries.

[0009] The third object of the present invention is to provide a battery and its negative electrode and negative electrode material.

[0010] Waste photovoltaic graphite is basically isostatically pressed graphite waste. It is different from other waste graphites such as waste battery graphite. It has a significantly higher tap density, the interlayer bonding is particularly tight, and it is difficult to remove impurities. In addition, its intrinsic physical and chemical structure is difficult to adapt to battery application requirements, and under strong impurity removal precursors, its structure may be further damaged, making it difficult to regenerate into graphite negative electrode active materials, especially difficult to obtain graphite active materials with excellent fast charging performance under high surface loads. Based on the above technical difficulties, there is no solution in the industry to regenerate graphite negative electrode materials from photovoltaic waste graphite. In response to this problem, the present invention has been studied in depth and provides the following improvement plan:

[0011] A method for preparing waste photovoltaic graphite-based regenerated graphite negative electrode active material, comprising the following steps:

[0012] Step (1):

[0013] The graphite block material from waste photovoltaic sources is crushed and sieved to obtain graphite powder, and then the graphite powder is subjected to a two-stage gradient gas change treatment to obtain pretreated graphite;

[0014] The two-stage gradient gas change treatment includes a first stage of heat preservation process in advance at atmosphere A and temperature T1, and a second stage of heat preservation process in which the gas is changed to atmosphere B and carried out at temperature T2; the atmosphere A is an oxidizing atmosphere, and the temperature T1 is 200-350°C; the atmosphere B is an atmosphere containing at least one of a F source component and a Cl source component, wherein T2 is 350-650°C, and T2 is greater than T1;

[0015] Step (2):

[0016] The pretreated graphite is dispersed in water for slurrying, and then a modifier having a structure of formula A is added, and a modification treatment is performed under the assistance of ultrasound, followed by solid-liquid separation and drying to obtain modified graphite;

[0017]

[0018] In formula A, X is C and Y is S; or X is S and Y is O; R is halogen, C1-C6 alkyl, substituted alkyl or alkylamino;

[0019] Step (3):

[0020] The modified graphite, the boron-containing modifier and the carbon source are dispersed in a solvent and then subjected to a spray granulation treatment to obtain particles;

[0021] Step (4):

[0022] The particles of step (3) are carbonized and then carbon coated to obtain the waste photovoltaic graphite-based regenerated graphite negative electrode active material.

[0023] In order to solve the problem that photovoltaic waste graphite is difficult to regenerate to form graphite negative electrode materials due to its own structural characteristics, the present invention innovatively pre-treats photovoltaic waste graphite with variable gas gradient treatment under the conditions, and then combines the modification of formula A with spray treatment assisted by a boron-containing modifier and subsequent carbonization and carbon coating treatment processes. This can unexpectedly achieve synergy, break through the physicochemical characteristics of photovoltaic waste graphite, and selectively remove electrochemical harmful impurities therein. Not only that, it can also optimize and repair its physicochemical structure to make it suitable for battery applications, especially for applications under high surface load conditions, thereby improving the liquid absorption and electrochemical properties of the regenerated graphite, especially improving its electrochemical properties under high surface load, especially fast charging performance.

[0024] In the present invention, the graphite block material from waste photovoltaic sources is derived from isostatically pressed graphite waste from the photovoltaic industry. As an optional solution, the fixed carbon content of the isostatically pressed graphite waste is above 90wt%, for example, 92-98wt%, and the degree of graphitization can be 85-95%.

[0025] In the present invention, the D50 of the graphite powder after crushing and sieving is 3 to 20 μm, and can further be 5 to 15 μm.

[0026] In the present invention, the two-stage gas change treatment and the joint control of the atmosphere and temperature in the process are helpful to break through the physical and chemical characteristics of waste photovoltaics, help to combine with other processes to selectively remove electrochemical harmful impurities therein, and also help to adjust its physical and chemical structure to make it suitable for battery applications, especially high-load application requirements.

[0027] In the present invention, the atmosphere A is a gas containing at least one gas a selected from the group consisting of air, oxygen and ozone.

[0028] Preferably, the atmosphere A also contains a diluent gas, and the diluent gas includes at least one of nitrogen and an inert gas.

[0029] Preferably, the content of gas a in the atmosphere A is above 0.5v%. For example, when gas a is air, the volume content of gas a in atmosphere A may be 50-100%. When gas a is oxygen, the volume content of gas a in atmosphere A may be 10-50%. When gas a is ozone, the volume content of gas a in atmosphere A may be 0.5-10%.

[0030] In the present invention, the temperature of the first stage of heat preservation may be 230-320°C, and further may be 250-300°C.

[0031] Preferably, the first stage of heat preservation treatment lasts for 1 to 6 hours, and can further be 2 to 4 hours.

[0032] In the present invention, after the first stage of heat preservation treatment, the temperature of the system is raised to temperature T2, and then the atmosphere is changed to atmosphere B to perform the second stage of heat preservation treatment.

[0033] In the present invention, in the atmosphere B, the F-containing source component and the Cl-containing source component are gas components containing the respective elements.

[0034] In the present invention, the atmosphere B is preferably an atmosphere containing F source components. The present invention shows that the preferred atmosphere can be further combined with other processes to further adapt to the requirements of photovoltaic waste graphite regeneration graphite active materials, and is conducive to obtaining graphite active materials with better performance.

[0035] Preferably, the F-containing source component includes at least one of fluorine gas, carbon tetrafluoride, nitrogen trifluoride, and sulfur hexafluoride.

[0036] In the present invention, the atmosphere B is also allowed to contain a diluent gas, and the diluent gas includes, for example, at least one of nitrogen and an inert gas.

[0037] In the present invention, the content of the F source component in the atmosphere B is 0.01-0.5v%, and can further be 0.1-0.3v%.

[0038] In the present invention, the temperature of the second insulation stage may be 380-580°C, and further may be 400-550°C.

[0039] Preferably, the second insulation time is 1 to 10 hours, further 3 to 6 hours.

[0040] In the present invention, in step (2), the liquid-to-solid ratio of the pretreated graphite and water is 1 to 10 ml / g, and can further be 3 to 6 ml / g.

[0041] Preferably, the formula A modifier includes formula A-1 and formula A-2;

[0042]

[0043] In the formula A-1, R is Cl, trifluoromethyl, dialkylamino or tert-butyl;

[0044] In the formula A-2, R is a dialkylamino group.

[0045] In the present invention, the modifier of formula A which is a combination of formula A-1 and formula A-2 can further achieve synergy, which can further adapt to the characteristics of photovoltaic waste graphite and give the battery-adaptive physicochemical characteristics of the negative electrode material regenerated from photovoltaic waste graphite, thereby further enhancing the electrochemical properties of the regenerated graphite active material.

[0046] In the present invention, in the modifier of formula A, the weight ratio of formula A-1 to formula A-2 is 1:0.1-10, and can further be 1:0.5-2.

[0047] Preferably, the weight ratio of graphite powder to modifier of formula A is 100:0.2-4, and can further be 100:1-2.

[0048] Preferably, the power of ultrasound is above 100W, preferably 100-600W.

[0049] Preferably, the modification treatment time is 10 to 30 minutes.

[0050] In the present invention, the boron-containing modifier includes one or more of boron oxide, boric acid, phenylboric acid, potassium trifluoroborate, methylboric acid, butylboric acid, lithium metaborate, 2,4-dichlorophenylboric acid, sodium tetraphenylborate, dilithium tetraborate, triethyl borate, potassium tetrafluoroborate, etc.

[0051] Preferably, the mass ratio of modified graphite to boron-containing modifier is 100:0.5-5; preferably 100:1-2.

[0052] Preferably, the carbon source includes one or more of citric acid, sucrose, glucose, polyethylene glycol, etc.

[0053] Preferably, the mass ratio of modified graphite to carbon source is 100:5-18, preferably 100:10-15.

[0054] Preferably, the solvent is one or more of water, ethanol, tetrahydrofuran, toluene and acetone.

[0055] There is no special requirement for the particle size after spraying, as long as it meets the battery application requirements, for example, it can be 5 to 18 μm.

[0056] In the present invention, the modified graphite, carbon source and boron-containing modifier are further sprayed together to solve the problems of large polarization of the regenerated active material due to large particle sharpness and unsatisfactory performance due to high compaction of the pole piece in the stage of regenerating the graphite active material of photovoltaic waste graphite.

[0057] In the present invention, the sprayed material is subjected to conventional carbonization and carbon coating treatment to obtain the regenerated graphite active material.

[0058] As an illustrative embodiment, in step (4), the carbonization process includes low-temperature carbonization and high-temperature carbonization processes, wherein the temperature of the low-temperature carbonization is 350-500°C; the insulation time at the low-temperature carbonization temperature is 4-8 hours; the temperature of the high-temperature carbonization process is 900-1500°C, and the time of the high-temperature carbonization is 4-8 hours.

[0059] In the present invention, the carbon coating process can be achieved based on conventional solid phase, liquid phase and gas phase carbon coating methods. In the present invention, the carbon coating method is a gas phase carbon deposition method.

[0060] The vapor phase carbon deposition method is, for example, to introduce an atomized or gasified carbon source into a temperature system that maintains high temperature carbonization, and perform a heat preservation carbon coating treatment.

[0061] A preferred step (4) of the present invention is: pre-carbonizing the particles of step (3) at low temperature in a protective atmosphere, then carbonizing them at high temperature, and then switching the atmosphere to a carbon source-containing atmosphere under the high temperature carbonization temperature conditions to perform gas phase carbon deposition treatment.

[0062] The carbon source-containing atmosphere may be an atmosphere containing at least one carbon source gas selected from the group consisting of alkanes, alkenes, alkynes, and aromatic hydrocarbons, and may further be one or more selected from the group consisting of methane, ethane, acetylene, and benzene.

[0063] In the present invention, at least one of hydrogen and diluent gas is allowed to exist in the carbon source-containing atmosphere.

[0064] Furthermore, the carbon source-containing atmosphere is a mixture of carbon source gas and hydrogen in a volume ratio of 1:1 to 5.

[0065] In the present invention, the carbon coating (carbon deposition) time may be 1 to 3 hours, and further may be 1.5 to 2 hours.

[0066] In the present invention, the protective atmosphere includes at least one of nitrogen and inert gas.

[0067] The present invention also provides a waste photovoltaic graphite-based regenerated graphite negative electrode active material prepared by the preparation method.

[0068] The preparation method of the present invention can endow the prepared recycled material with special physicochemical characteristics, and the recycled material with the characteristics can unexpectedly exhibit excellent electrochemical properties, especially can significantly improve its electrochemical properties under high surface load.

[0069] The present invention also provides an application of the waste photovoltaic graphite-based regenerated graphite negative electrode active material, which is used as a negative electrode active material for preparing an alkali metal ion battery.

[0070] In the present invention, the alkali metal ion battery includes a lithium ion battery or a sodium ion battery.

[0071] In the present invention, in the alkali metal ion battery, except for the negative electrode active material of the present invention, other components and parts can be conventional.

[0072] The present invention also provides a negative electrode of an alkali metal ion battery, comprising a current collector and a negative electrode material composited on the surface thereof, wherein the negative electrode material comprises a negative electrode active material, a binder and a conductive agent, and the negative electrode active material comprises the waste photovoltaic graphite-based recycled graphite negative electrode active material prepared by the preparation method of the present invention.

[0073] In the present invention, in the negative electrode, except for the waste photovoltaic graphite-based regenerated graphite negative electrode active material described in the present invention, other ingredients and components can be conventional.

[0074] For example, in the negative electrode active material described in the present invention, the content of the waste photovoltaic graphite-based regenerated graphite negative electrode active material is above 80wt.%; further, it can be waste photovoltaic graphite-based regenerated graphite negative electrode active material.

[0075] In the present invention, the binder and the conductive agent in the negative electrode material can be conventional in the field of ion batteries. In addition, the content of the negative electrode active material in the negative electrode material can be 80-95wt%.

[0076] In the present invention, the pole piece compaction density of the waste photovoltaic graphite-based regenerated graphite negative electrode active material is 1.8-2 g / cm 3 , and further can be 1.82 to 1.89 g / cm 3 The negative electrode of the present invention, thanks to the use of the waste photovoltaic graphite-based regenerated graphite negative electrode active material, can still show excellent fast charging performance under high surface load.

[0077] The present invention also provides an alkali metal ion battery, which comprises the negative electrode of the present invention.

[0078] The battery of the present invention, except for the waste photovoltaic graphite-based regenerated graphite negative electrode active material of the present invention, other components and parts can be conventional.

[0079] Beneficial Effects

[0080] The present invention innovatively subjects photovoltaic waste graphite to a variable gas gradient treatment under the conditions in advance, and then combines the modification of formula A and the spray treatment assisted by a boron-containing modifier with subsequent carbonization and carbon coating treatment processes. This unexpectedly achieves synergy, can break through the physical and chemical characteristics of photovoltaic waste graphite, and selectively remove electrochemical harmful impurities therein. Not only that, it can also optimize and repair its physical and chemical structure to make it suitable for battery applications, especially for applications under high surface load conditions, thereby improving the performance of the regenerated graphite, especially improving its electrochemical performance under high surface load. BRIEF DESCRIPTION OF THE DRAWINGS

[0081] Figure 1 This is the SEM image of the regenerated graphite active material in Example 1. DETAILED DESCRIPTION

[0082] The specific steps of the present invention are described below by way of examples. It should be understood that these examples are only for illustrating the present invention and are not intended to limit the scope of the present invention in any way. Various processes and methods not described in detail in the present invention are conventional methods known in the art.

[0083] The block graphite is isostatic graphite waste retired from the photovoltaic industry. The fixed carbon content of the raw material is 94.2% and the graphitization degree is 90.4%.

[0084] Example 1

[0085] Step 1: crush the photovoltaic waste block graphite and sieve it into graphite powder (D50 is 5.4±0.1μm);

[0086] Step 2: Place the powder obtained in step 1 in an atmosphere furnace, firstly perform the first heat preservation treatment under atmosphere A (air) and temperature T1 (250°C) (heat preservation time t1 is 3h), then heat to temperature T2 (400°C) at a heating rate of 10°C / min, switch the atmosphere to atmosphere B (0.1v% F2-Ar mixed gas) and perform the second heat preservation (heat preservation time t2 is 4h), then perform air flow milling treatment, sieve, and obtain pretreated graphite;

[0087] Step 3: The obtained pretreated graphite powder is slurried with water (liquid-to-solid ratio is 5 ml / g), and then Formula A (in this case, Formula a, which is a compound of Formula A-1 in which R is trifluoromethyl, Formula A is a pretreated graphite powder with a weight ratio of 1:100) is added, followed by ultrasonic treatment (100 W) for 15 min, followed by solid-liquid separation, water washing, drying, and breaking up to obtain modified graphite;

[0088] Step 4: The boron compound (boron oxide), the carbon source (sucrose), and the modified graphite are uniformly mixed in a weight ratio of 1:10:100, dispersed in water (liquid-solid ratio of 5 ml / g), and spray granulated to obtain graphite spray particles (particle size of 7±1 μm);

[0089] Step 5:

[0090] The graphite spray particles are placed in an atmosphere furnace, and are pre-heated in an Ar atmosphere at a temperature of 400±20°C (marked as T3) for low-temperature carbonization for 6 hours, and then heat-treated at a temperature of 1000±20°C (marked as T4) for high-temperature carbonization for 6 hours. The atmosphere is then switched to a mixed atmosphere of methane and hydrogen (volume ratio of 1:4), and after heat deposition for 2 hours, the particles are cooled in the furnace to obtain the regenerated graphite material.

[0091] Example 2

[0092] Compared with Example 1, the only difference is that the conditions of step 1 are changed, that is, the fixed carbon content of the waste photovoltaic graphite is 93.8%, and the degree of graphitization is 89.2%. After crushing, it is sieved to obtain graphite powder (D50 is 12.5±0.1μm). Other operations and parameters are the same as in Example 1.

[0093] Example 3

[0094] Compared with Example 1, the only difference is that the conditions of step 2 are changed, and the experimental groups are:

[0095] Group A: Atmosphere A is a 30v% oxygen-argon mixture, the temperature T1 is 300°C, and the time t1 is 2h; Atmosphere B is a 0.3v% F2-Ar atmosphere, the temperature T2 is 550°C, and the time t2 is 3h.

[0096] Group B: F2 in atmosphere B was replaced with an equal volume of Cl2;

[0097] Other operations and parameters are the same as in Example 1.

[0098] Example 4

[0099] Compared with Example 1, the only difference is that the conditions in step 3 are changed. The experimental groups are:

[0100] Group A: Formula A is a compound of Formula b, which is a compound of Formula A-2 wherein R is dimethylamino;

[0101] Group B: Formula A is a composite of Formula a and Formula b in a weight ratio of 1:1;

[0102] Group C: The obtained pretreated graphite powder was slurried with water (liquid-to-solid ratio was 6 ml / g), and then Formula A (in this case, Formula A is the weight ratio of pretreated graphite powder is 2:100) was added, and then ultrasonic (200W) treatment was performed for 10 min, and then solid-liquid separation, water washing, drying, and dispersion were performed to obtain modified graphite;

[0103] Other operations and parameters are the same as in Example 1.

[0104] Example 5

[0105] Compared with Example 1, the only difference is that the operation of step 4 is changed, specifically: the boron compound (boric acid), the carbon source (glucose), and the above-mentioned modified graphite are uniformly mixed in a weight ratio of 1.5:15:100, dispersed in water (liquid-solid ratio of 8 ml / g), and spray granulated to obtain graphite spray particles. Other operations and parameters are the same as in Example 1.

[0106] Example 6

[0107] Compared with Example 1, the only difference is that the conditions of step 5 are changed, specifically, the temperature of low-temperature carbonization is 450±20°C, the carbonization time is 5h, the temperature of high-temperature carbonization is 1100±20°C, and the high-temperature carbonization time is 5h; the mixed atmosphere in the deposition stage is acetylene-hydrogen (volume ratio is 1:1), and the deposition time is 1.5h. Other operations and parameters are the same as in Example 1.

[0108] Comparative Example 1

[0109] Compared with Example 1, the only difference is that the atmosphere A is replaced by Ar, and the other operations and parameters are the same as those in Example 1.

[0110] Comparative Example 2

[0111] Compared with Example 1, the only difference is that the atmosphere B is replaced by Ar, and the other operations and parameters are the same as those in Example 1.

[0112] Comparative Example 3

[0113] Compared with Example 1, the only difference is that in step 2, the processing order of the first insulation stage and the second insulation stage is exchanged, that is, the powder in step 1 is preliminarily subjected to insulation treatment t2 under atmosphere B and temperature T2, then cooled to temperature T1, and then the atmosphere is switched to atmosphere A for insulation treatment t1. Other operations and parameters are the same as in Example 1.

[0114] Comparative Example 4

[0115] Compared with Example 1, the only difference is that in step 3, ultrasound assistance is not performed, and other operations and parameters are the same as Example 1.

[0116] Comparative Example 5

[0117] Compared with Example 1, the only difference is that in step 3, Formula A is not added, and other operations and parameters are the same as Example 1.

[0118] Comparative Example 6

[0119] Compared with Example 1, the only difference is that in step 4, no boride is added, and other operations and parameters are the same as Example 1.

[0120] Comparative Example 7

[0121] Compared with Example 1, the only difference is that in step 4, vacuum air drying is directly performed after slurrying without spraying treatment. Other operations and parameters are the same as in Example 1.

[0122] 3. Test:

[0123] 1. Electrochemical performance test

[0124] The regenerated graphite negative electrode active material, binder (LA-133, CMC) and super carbon black of each case were uniformly mixed in a mass ratio of 92:3:3:2, and then water was added to stir to make a uniform slurry, which was coated on a copper foil and placed in a vacuum dryer at 120 ° C for 12 h to obtain a graphite compaction density of 1.86 ± 0.05 g / cm 3 Electrode sheet (graphite negative electrode sheet).

[0125] A CR2032 button battery case was used, the obtained graphite negative electrode sheet was used as the working electrode, the metal lithium sheet was used as the counter electrode, a Celgard 2400 diaphragm was used, nickel foam was used as the counter electrode side current collector, and a solution of ethylene carbonate + dimethyl carbonate + diethyl carbonate (EC+DMC+DEC, 1:1:1) containing 1M LiPF6 was used as the electrolyte. The cells were assembled in a glove box under an argon atmosphere, and then compressed and packaged using a sealing machine to obtain a button lithium battery.

[0126] The battery cycle performance was tested at room temperature, with a test voltage range of 0.01V to 1.5V and a test rate of 0.1C and 6C. The results are shown in Table 1:

[0127] Table 1

[0128]

[0129] 2. Liquid absorption performance test

[0130] 50 μL of electrolyte (ethylene carbonate + dimethyl carbonate + diethyl carbonate (EC+DMC+DEC, 1:1:1) solution containing 1M LiPF6) was dropped onto the graphite electrode in each case, and the time it took for the electrolyte to be completely absorbed by the electrode was recorded. The shorter the time, the better the liquid absorption performance of the electrode.

[0131] sample Absorption time (min) Example 1 1.14 Example 2 1.09 Example 3A 1.11 Example 3B 1.24 Example 4A 1.09 Example 4B 1.00 Example 4C 1.10 Example 5 1.14 Example 6 1.07 Comparative Example 1 2.62 Comparative Example 2 2.24 Comparative Example 3 2.77 Comparative Example 4 2.66 Comparative Example 5 3.02 Comparative Example 6 2.75 Comparative Example 7 2.97

[0132] It can be seen from the above table that even under high compaction conditions, the electrode sheet prepared from the material obtained in the example still has good liquid absorption performance, can improve the overvoltage problem caused by the high compaction density of the traditional graphite negative electrode, and can meet the requirements of high-energy-density lithium-ion batteries for high-performance graphite negative electrodes.

Claims

1. A method for preparing waste photovoltaic graphite-based regenerated graphite negative electrode active material, characterized in that the steps include: Step (1): The graphite block material from waste photovoltaic sources is crushed and sieved to obtain graphite powder, and then the graphite powder is subjected to a two-stage gradient gas change treatment to obtain pretreated graphite; The two-stage gradient gas change treatment includes a first stage of heat preservation process in advance at atmosphere A and temperature T1, and a second stage of heat preservation process in which the gas is changed to atmosphere B and carried out at temperature T2; the atmosphere A is an oxidizing atmosphere, and the temperature T1 is 200-350°C; the atmosphere B is an atmosphere containing at least one of a F source component and a Cl source component, wherein T2 is 350-650°C, and T2 is greater than T1; Step (2): The pretreated graphite is dispersed in water for slurrying, and then a modifier having a structure of formula A is added, and a modification treatment is performed under the assistance of ultrasound, followed by solid-liquid separation and drying to obtain modified graphite; In formula A, X is C and Y is S; or X is S and Y is O; R is halogen, C1-C6 alkyl, substituted alkyl or alkylamino; Step (3): The modified graphite, the boron-containing modifier and the carbon source are dispersed in a solvent and then subjected to a spray granulation treatment to obtain particles; Step (4): The particles of step (3) are carbonized and then carbon-coated to obtain the waste photovoltaic graphite-based regenerated graphite negative electrode active material.

2. The preparation method according to claim 1, characterized in that The graphite block material from waste photovoltaic sources is derived from isostatically pressed graphite waste from the photovoltaic industry; Preferably, the fixed carbon content of the static graphite waste is above 90wt%; the degree of graphitization can be 85-95%; Preferably, the D50 of the graphite powder after crushing and screening is 3 to 20 μm.

3. The preparation method according to claim 1, characterized in that: The atmosphere A is a gas containing at least one gas a selected from air, oxygen and ozone; Preferably, the atmosphere A also contains a diluent gas, and the diluent gas includes at least one of nitrogen and an inert gas; Preferably, in the atmosphere A, the content of gas a is above 0.5v%; Preferably, the first stage of heat preservation treatment lasts for 1 to 6 hours; Preferably, the atmosphere B is an atmosphere containing a F source component; Preferably, the F-containing source component includes at least one of fluorine gas, carbon tetrafluoride, nitrogen trifluoride, and sulfur hexafluoride; Preferably, the content of F source components in the atmosphere B is 0.01-0.5v%; Preferably, the second insulation time is 1 to 10 hours.

4. The preparation method according to claim 1, characterized in that: In step (2), the liquid-to-solid ratio of the pretreated graphite and water is 1 to 10 ml / g; Preferably, the formula A modifier includes formula A-1 and formula A-2; In the formula A-1, R is Cl, trifluoromethyl, dialkylamino or tert-butyl; In the formula A-2, R is a dialkylamino group; Preferably, in the modifier of formula A, the weight ratio of formula A-1 to formula A-2 is 1:0.1 to 10; Preferably, the weight ratio of graphite powder to modifier of formula A is 100:0.2-4; Preferably, the power of ultrasound is above 100W, preferably 100 to 600W; Preferably, the modification treatment time is 10 to 30 minutes.

5. The preparation method according to claim 1, characterized in that: The boron-containing modifier includes one or more of boron oxide, boric acid, phenylboric acid, potassium trifluoroborate, methylboric acid, butylboric acid, lithium metaborate, 2,4-dichlorophenylboric acid, sodium tetraphenylborate, dilithium tetraborate, triethyl borate, potassium tetrafluoroborate, etc.; Preferably, the mass ratio of modified graphite to boron-containing modifier is 100:0.5-5; Preferably, the carbon source includes one or more of citric acid, sucrose, glucose, polyethylene glycol, etc.; Preferably, the mass ratio of modified graphite to carbon source is 100:5-18; Preferably, the solvent is one or more of water, ethanol, tetrahydrofuran, toluene, and acetone; Preferably, the particle size after spraying is 5 to 18 μm.

6. The preparation method according to claim 1, characterized in that: In step (4), the carbonization process includes low-temperature carbonization and high-temperature carbonization, wherein the temperature of the low-temperature carbonization is 350-500°C; the holding time at the low-temperature carbonization temperature is 4-8 hours; the temperature of the high-temperature carbonization process is 900-1500°C, and the holding time of the high-temperature carbonization is 4-8 hours; Preferably, the carbon coating method is a gas phase carbon deposition method.

7. A waste photovoltaic graphite-based regenerated graphite negative electrode active material prepared by the preparation method according to any one of claims 1 to 6.

8. An application of waste photovoltaic graphite-based regenerated graphite negative electrode active material prepared by the preparation method according to any one of claims 1 to 6, characterized in that: It is used as negative electrode active material to prepare alkali metal ion batteries; Preferably, the alkali metal ion battery comprises a lithium ion battery or a sodium ion battery.

9. A negative electrode of an alkali metal ion battery, comprising a current collector and a negative electrode material composited on the surface of the current collector, wherein the negative electrode material comprises a negative electrode active material, a binder and a conductive agent, characterized in that: The negative electrode active material comprises the waste photovoltaic graphite-based recycled graphite negative electrode active material prepared by the preparation method according to any one of claims 1 to 6; Preferably, in the negative electrode active material, the content of the waste photovoltaic graphite-based recycled graphite negative electrode active material is above 80wt.%; Preferably, in the negative electrode, the pole piece compaction density of the waste photovoltaic graphite-based recycled graphite negative electrode active material is 1.8-2 g / cm 3 , and further can be 1.82 to 1.89 g / cm 3 .

10. An alkali metal ion battery, characterized in that: The negative electrode according to claim 9 is included.

Citation Information

Patent Citations

  • Graphite powder of lithium ionic cell cathode and preparation thereof

    CN101323447A

  • High-conductivity remote disordered carbon-coated graphite negative electrode material and preparation and application thereof

    CN116135783A

  • Preparation method of hard carbon negative electrode material, hard carbon negative electrode material and application of hard carbon negative electrode material

    CN116854072A

  • Carbon-coated graphite material taking waste batteries as raw materials and preparation method of carbon-coated graphite material

    CN118486939A

  • Natural graphite-based modified composite material, preparation method therefor, and lithium ion battery comprising modified composite material

    US20200266443A1

Cited By

  • Method for preparing high-purity graphite by roasting waste graphite with sodium carbonate-sodium borate

    CN120057916A

  • Waste graphite regenerated material as well as preparation and application thereof

    CN120097336A