Molecular sieve as well as preparation method and application thereof
By developing a one-dimensional 16-membered ring pore structure molecular sieve DNL-11, the problem of lack of stable super-large pore structure in existing phosphorus-aluminum molecular sieve is solved, and high water adsorption and stability are achieved, and used in water adsorbents are improved. Performance in adsorption separation and energy storage applications.
Patent Information
- Application Number
- CN202310526307.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-10
AI Technical Summary
The lack of stable ultra-large pore structures in the existing phosphoaluminum molecular sieve family limits the understanding and application of its adsorption and catalytic properties.
A new one-dimensional 16-membered ring channel structure molecular sieve DNL-11 was developed. By using phosphorus source, aluminum source, silicon source, organic template agent and fluoride, materials such as fluoride were prepared with high water adsorption. Molecular sieve and ensure its stability through specific synthesis steps and conditions.
A one-dimensional 16-membered ring-pore molecular sieve DNL-11 with high water adsorption and stability was successfully synthesized. It is used for water adsorbents, with a water absorption of more than 350mg/g, and provides new materials for adsorption separation and storage. Can be applied.
Smart Images

Figure BDA0004223206260000021 
Figure BDA0004223206260000061 
Figure BDA0004223206260000071
Abstract
Description
Technical Field
[0001] The present application relates to a molecular sieve and a preparation method thereof and application in a water adsorbent. The applicant names it DNL-11, which belongs to the field of molecular sieves. Background Art
[0002] Phosphoaluminum molecular sieve is a phosphate aluminate with regular pores or cage-like structures composed of phosphorus-oxygen tetrahedrons and aluminum-oxygen tetrahedrons with oxygen vertices interconnected. It was successfully developed by Union Carbide Corporation (UCC) in 1982, greatly expanding the molecular sieve family and becoming a milestone in the history of molecular sieves. There are many members in the phosphate aluminum molecular sieve family, mainly because the phosphorus or aluminum in the phosphate aluminum molecular sieve can be easily replaced by metal elements such as Si or Mg isomorphously to form silicoaluminophosphate molecular sieve (SAPO) and metal silicoaluminophosphate molecular sieve (MeAPO). At present, more than a dozen metal elements have been integrated into the phosphate aluminum molecular sieve family, and these molecular sieves have been widely used in the fields of adsorption and catalysis.
[0003] Phosphate-aluminate molecular sieves are generally synthesized by hydrothermal method. Since RM Barrer and PJ Denny introduced organic templates into the hydrothermal synthesis system of molecular sieves in 1961, the design, synthesis and introduction of organic templates have greatly increased the number of artificially synthesized zeolites. However, up to now, there are only 46 types of phosphate-aluminate molecular sieves published by IZA, and the potential and prospects for the development of phosphate-aluminate molecular sieves are still very huge.
[0004] Since the 19th century, researchers have been seeking to break through the limitation of 12-membered rings of molecular sieves, and have successfully made breakthroughs in the phosphorus-aluminum molecular sieve system. VFI is the first one-dimensional 18-membered ring super-large pore phosphorus-aluminum molecular sieve, but it is unstable when heated and converted into AlPO-8. And until today, there is only one IFO structure of fully connected phosphorus-aluminum molecular sieves with super-large pores and stability, so we still lack understanding of the pore properties of super-large pore phosphorus-aluminum molecular sieves. Summary of the invention
[0005] According to the first aspect of the present application, a molecular sieve DNL-11 having a one-dimensional 16-membered ring channel is provided, which is of great significance for understanding the adsorption of phosphate aluminum molecular sieves and the catalytic and adsorption properties of ultra-large pore silicon phosphate aluminum molecular sieves.
[0006] The molecular sieve has a one-dimensional 16-membered ring channel;
[0007] The X-ray powder diffraction of the molecular sieve has diffraction peaks at least at the following positions.
[0008]
[0009] The chemical formula of the molecular sieve is (H2O) x R2(Siy Al 8-y P8O 32 F2),
[0010] Where x = 0 to 10.0, y = 0 to 2.0;
[0011] R is a positively charged group of 4-pyrrolidinylpyridine.
[0012] According to another aspect of the present application, a method for synthesizing the above-mentioned molecular sieve is provided, comprising at least the following steps:
[0013] (1) mixing water, a phosphorus source, an aluminum source, a silicon source, an organic template, a mineralizer and a solvent to obtain a mixture;
[0014] (2) crystallizing the mixture obtained in (1) in a closed reaction vessel to obtain a crystallized product;
[0015] (3) calcining the crystallized product to remove the template and obtain the molecular sieve.
[0016] Optionally, the method comprises the following steps:
[0017] (1) under stirring conditions, a phosphorus source, an aluminum source, a silicon source, an organic template, water, a fluoride and an alcohol are uniformly mixed in proportion to form a reaction gel;
[0018] (2) transferring the reaction gel into a stainless steel reactor and crystallizing it at 130-200° C. for 1-15 days under sealed conditions;
[0019] (3) washing and drying the crystallized product to obtain DNL-11;
[0020] The organic template is 4-pyrrolidinopyridine.
[0021] The phosphorus source is selected from phosphoric acid and / or phosphorus pentoxide;
[0022] The aluminum source is selected from at least one of pseudo-boehmite, aluminum hydroxide or aluminum isopropoxide;
[0023] The silicon source is selected from at least one of silica sol, ethyl orthosilicate, tetramethoxysilane or white carbon black;
[0024] The mineralizer is selected from HF and / or NH4F; the fluoride ions therein are effective.
[0025] The solvent is selected from alcohols.
[0026] Optionally, the alcohol is selected from at least one of cyclohexanol, ethylene glycol, diethylene glycol and triethylene glycol.
[0027] The molar composition of the mixture is aR: bHF: cH3PO4: qSiO2: Al2O3: mROH: nH2O;
[0028] Wherein, R represents the positively charged group of the organic template;
[0029] a=0.1~5.0;
[0030] b = 1.0 to 5.0;
[0031] c = 0.5-5.0;
[0032] q = 0 to 1.0;
[0033] m = 0 to 100;
[0034] n=5~100.
[0035] Optionally, a is independently selected from any value among 0.1, 0.2, 0.5, 1.0, 1.2, 1.6, 1.9, 2.0, 2.4, 2.5, 2.8, 3.1, 3.3, 3.8, 3.9, 4.0, 4.2, 4.3, 4.6, 4.8, 5.0 or any range therebetween.
[0036] Optionally, b is independently selected from any value among 1.0, 1.2, 1.5, 1.8, 2.0, 2.1, 2.3, 2.4, 2.8, 3.0, 3.1, 3.2, 3.4, 3.6, 4.0, 4.2, 4.5, 4.8, 5.0 or any range therebetween.
[0037] Optionally, c is independently selected from any value among 0.5, 0.8, 1.0, 1.1, 1.3, 1.6, 1.8, 2.0, 2.4, 2.6, 3.0, 3.3, 4.0, 4.2, 4.6, 5.0, or any range therebetween.
[0038] Optionally, q is independently selected from any value among 0, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, or any range between two values.
[0039] Optionally, m is independently selected from any value among 0, 10, 15, 20, 30, 40, 50, 60, 70, 80, 90, 100, or any range therebetween.
[0040] Optionally, n is independently selected from any value among 5, 10, 20, 25, 30, 50, 60, 70, 80, 90, 100, or any range therebetween.
[0041] The crystallization temperature is 130-200°C;
[0042] Optionally, the crystallization temperature is independently selected from any value of 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, or any range therebetween.
[0043] The crystallization time is 1 to 15 days.
[0044] Optionally, the crystallization time is independently selected from any value among 1d, 2d, 3d, 4d, 5d, 6d, 7d, 8d, 9d, 10d, 12d, 13d, 14d, 15d, or any range between two of them.
[0045] Optionally, the crystallization temperature is 150-200°C.
[0046] Optionally, the crystallization temperature is independently selected from any value among 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, or any range therebetween.
[0047] According to another aspect of the present application, there is provided an application of the above-mentioned molecular sieve as a water adsorption material.
[0048] According to another aspect of the present application, a water adsorbent is provided, wherein the water adsorbent contains the above-mentioned molecular sieve or the molecular sieve prepared by the above-mentioned preparation method.
[0049] The water adsorbent is used for absorbing water and storing energy.
[0050] The water adsorbent can absorb water up to 350 mg / g or more.
[0051] The beneficial effects of this application include:
[0052] 1) This application synthesizes a new type of framework structure molecular sieve.
[0053] 2) The preparation method provided in this application has a simple synthesis process and strong operability.
[0054] 3) The novel framework structure molecular sieve prepared in the present application can be used for adsorption separation and has high water adsorption capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 It is the X-ray powder diffraction spectrum (XRD) of the product obtained in Example 1 of the present application.
[0056] Figure 2 This is a scanning electron microscope image (SEM) of the product obtained in Example 1 of the present application.
[0057] Figure 3 It is the water absorption isotherm adsorption curve of DNL-11 in Example 10 of the present application. DETAILED DESCRIPTION
[0058] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0059] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0060] The analysis method in the examples of this application is as follows:
[0061] The sample phase analysis was carried out by X-ray powder diffraction (XRD) analysis. The instrument used was an X'Pert PRO X-ray diffractometer from PANalytical of the Netherlands, using a Cu target and a Kα light source. Tested under 40KV voltage and 40mA current.
[0062] The composition of the samples was determined by X-ray fluorescence spectroscopy (XRF) analysis using a Magix-601 X-ray fluorescence spectrometer from Philips.
[0063] The sample morphology was analyzed by scanning electron microscopy (SEM), and the instrument used was: Hitachi SU8020 field emission scanning electron microscope.
[0064] The samples were thermally analyzed using a TA Q-600 thermal analyzer at a heating rate of 10°C / min from room temperature to 900°C.
[0065] The water vapor adsorption test of the samples was carried out using the BSD-VVS multi-station gravimetric gas vapor adsorption instrument produced by Bester Company at a P / P0 of 0.8 and a temperature of 25°C.
[0066] cRED data were collected on a JEOL 2100Plus transmission electron microscope equipped with an EMSIS GmbH camera and an ASI Cheetah120 detector.
[0067] Example 1 Preparation of Sample 1
[0068] 0.524g of orthophosphoric acid (85%) was added to 10.372g of triethylene glycol and mixed and stirred. Then 0.952g of aluminum triisopropoxide (98%) was added and stirred until uniform. Then 1.037g of 4-pyrrolidinopyridine (98%) was added and stirred vigorously (500rpm) to mix uniformly. Finally, 0.11g of hydrofluoric acid was added to obtain an initial gel mixture. The mixture was transferred to a stainless steel autoclave and statically crystallized at 200°C for 72 hours under autogenous pressure. After the crystallization, the solid product was centrifuged, washed, and dried in air at 100°C to obtain a white powder product. The product was confirmed to be DNL-11 by X-ray powder diffraction and was recorded as sample 1. The X-ray powder diffraction pattern (XRD) of sample 1 is shown as follows: Figure 1 As shown in the scanning electron microscope (SEM) Figure 2 As shown in the figure, the morphology of sample 1 is stick-shaped, with a size of 200nm to 200μm. At the same time, the morphology of the molecular sieve in the SEM image is uniform, and the synthesized molecular sieve does not contain other phases, reflecting the high purity of the molecular sieve. The elemental composition of sample 1 obtained by XRF analysis and thermal analysis normalization is: (H2O)8R2·(P8Al8O 32 F2) wherein R is 4-pyrrolidinylpyridine.
[0069] The X-ray powder diffraction characteristics of sample 1 are shown in Table 1:
[0070]
[0071]
[0072] Example 2 Preparation of Sample 2
[0073] 0.532g of orthophosphoric acid (85%) was added to 10.373g of triethylene glycol and mixed and stirred, and then 0.949g of aluminum triisopropoxide (98%) was added and stirred until uniform, and then 1.038g of 4-pyrrolidinopyridine (98%) was added and stirred vigorously (500rpm) to mix uniformly, and finally 0.57g of hydrofluoric acid was added to obtain an initial gel mixture. The mixture was transferred to a stainless steel autoclave and statically crystallized at 200°C for 72 hours under autogenous pressure. After the crystallization, the solid product was centrifuged, washed, and dried in air at 100°C to obtain a white powder product. The product was confirmed to be DNL-11 by X-ray powder diffraction and recorded as sample 2. The X-ray powder diffraction pattern (XRD) and scanning electron microscope (SEM) of sample 2 were similar to those of sample 1.
[0074] Example 3 Preparation of Sample 3
[0075] 0.278g of orthophosphoric acid (85%) was added to 10.38g of triethylene glycol and mixed and stirred, and then 0.95g of aluminum triisopropoxide (98%) was added and stirred until uniform, and then 1.037g of 4-pyrrolidinopyridine (98%) was added and stirred vigorously (500rpm) to mix uniformly, and finally 0.34g of hydrofluoric acid was added to obtain an initial gel mixture. The mixture was transferred to a stainless steel autoclave and statically crystallized at 200°C for 72 hours under autogenous pressure. After the crystallization, the solid product was centrifuged, washed, and dried in air at 100°C to obtain a white powder product. The product was confirmed to be DNL-11 by X-ray powder diffraction and recorded as sample 3. The X-ray powder diffraction pattern (XRD) and scanning electron microscope (SEM) of sample 3 were similar to those of sample 1.
[0076] Example 4 Preparation of Sample 4
[0077] 1.051 g of orthophosphoric acid (85%) was added to 10.381 g of triethylene glycol and mixed and stirred, and then 0.95 g of aluminum triisopropoxide (98%) was added and stirred until uniform, and then 1.036 g of 4-pyrrolidinopyridine (98%) was added and vigorously stirred (500 rpm) to mix uniformly, and finally 0.37 g of hydrofluoric acid was added to obtain an initial gel mixture. The mixture was transferred to a stainless steel autoclave and statically crystallized at 200° C. for 72 hours under autogenous pressure. After the crystallization, the solid product was centrifuged, washed, and dried in air at 100° C. to obtain a white powder product. The product was confirmed to be DNL-11 by X-ray powder diffraction and recorded as sample 4. The X-ray powder diffraction pattern (XRD) and scanning electron microscope (SEM) of sample 4 were similar to those of sample 1.
[0078] Example 5 Preparation of Sample 5
[0079] 0.685g of orthophosphoric acid (85%) was added to 9.495g of diethylene glycol and mixed and stirred, and then 1.217g of aluminum triisopropoxide (98%) was added and stirred until uniform, and then 1.041g of 4-pyrrolidinopyridine (98%) was added and stirred vigorously (500rpm) to mix uniformly, and finally 0.34g of hydrofluoric acid was added to obtain an initial gel mixture. The mixture was transferred to a stainless steel autoclave and statically crystallized at 200°C for 72 hours under autogenous pressure. After the crystallization, the solid product was centrifuged, washed, and dried in air at 100°C to obtain a white powder product. The product was confirmed to be DNL-11 by X-ray powder diffraction and recorded as sample 5. The X-ray powder diffraction pattern (XRD) and scanning electron microscope (SEM) of sample 5 were similar to those of sample 1.
[0080] Example 6 Preparation of Sample 6
[0081] 1.093g of orthophosphoric acid (85%) was added to 8.932g of ethylene glycol and mixed and stirred, and then 1.975g of aluminum triisopropoxide (98%) was added and stirred until uniform, and then 2.152g of 4-pyrrolidinopyridine (98%) was added and vigorously stirred (500rpm) to mix uniformly, and finally 1.186g of hydrofluoric acid was added to obtain an initial gel mixture. The mixture was transferred to a stainless steel autoclave and statically crystallized at 200°C for 72 hours under autogenous pressure. After the crystallization was completed, the solid product was centrifuged, washed, and dried in air at 100°C to obtain a white powder product. The product was confirmed to be DNL-11 by X-ray powder diffraction and recorded as sample 6. The X-ray powder diffraction pattern (XRD) and scanning electron microscope (SEM) of sample 6 were similar to those of sample 1.
[0082] Example 7 Preparation of Sample 7
[0083] 0.673g of orthophosphoric acid (85%) was added to 9.043g of ethylene glycol and mixed and stirred, and then 1.215g of aluminum triisopropoxide (98%) was added and stirred until uniform, and then 1.324g of 4-pyrrolidinopyridine (98%) was added and stirred vigorously (500rpm) to mix uniformly, and finally 0.438g of hydrofluoric acid was added to obtain an initial gel mixture. The mixture was transferred to a stainless steel autoclave and statically crystallized at 200°C for 72 hours under autogenous pressure. After the crystallization, the solid product was centrifuged, washed, and dried in air at 100°C to obtain a white powder product. The product was confirmed to be DNL-11 by X-ray powder diffraction and recorded as sample 7. The X-ray powder diffraction pattern (XRD) and scanning electron microscope (SEM) of sample 7 were similar to those of sample 1.
[0084] Example 8 Preparation of Sample 8
[0085] 0.528g of orthophosphoric acid (85%) was added to 10.382g of triethylene glycol and 1.363g of water, and the mixture was stirred. Then 0.95g of aluminum triisopropoxide (98%) was added, and the mixture was stirred until uniform. Then 1.039g of 4-pyrrolidinopyridine (98%) was added, and the mixture was stirred vigorously (500rpm) and mixed uniformly. Finally, 0.336g of hydrofluoric acid was added to obtain an initial gel mixture. The mixture was transferred to a stainless steel autoclave, and statically crystallized at 200°C for 72 hours under autogenous pressure. After the crystallization, the solid product was centrifuged, washed, and dried in air at 100°C to obtain a white powder product. The product was confirmed to be DNL-11 by X-ray powder diffraction, and was recorded as sample 8. The X-ray powder diffraction pattern (XRD) and scanning electron microscope (SEM) of sample 8 were similar to those of sample 1.
[0086] Example 9 Structural Analysis
[0087] Continuous rotation electron diffraction (cRED) tests were performed on samples 1-8. The structural analysis results showed that DNL-11 crystallized in the monoclinic system with a P21 space group. The unit cell parameters obtained by structural refinement were β = 105.791. Information about the molecular sieve framework is available.
[0088] Example 10 DNL-11 is used for adsorption separation
[0089] This example is used to illustrate the use of DNL-11 as a water adsorbent. However, the molecular sieve of the present application is not limited to being used for water adsorption.
[0090] The samples obtained in Examples 1-8 were placed in the adsorption instrument for pretreatment. The pretreatment conditions were heating at 250°C to constant weight; then a constant temperature water bath was used to stabilize the temperature at 25°C and the water vapor adsorption test was started. Typical experimental results are shown in Figure 3 . Figure 3 The experimental results show that when P / P0 is 0.8, the water vapor adsorption capacity is 356.126 mg / g. Other samples have achieved similar results.
[0091] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A molecular sieve, characterized in that: The molecular sieve has a one-dimensional 16-membered ring channel; The X-ray powder diffraction of the molecular sieve has diffraction peaks at least at the following positions.
2. The method according to claim 1, characterized in that: The chemical formula of the molecular sieve is (H2O) x R2(Si y Al 8-y P8O 32 F2), Where x = 0 to 10.0, y = 0 to 2.0; R is a positively charged group of 4-pyrrolidinylpyridine.
3. A method for synthesizing a molecular sieve according to any one of claims 1 or 2, characterized in that: At least the following steps are included: (1) mixing water, a phosphorus source, an aluminum source, a silicon source, an organic template, a mineralizer and a solvent to obtain a mixture; (2) crystallizing the mixture obtained in (1) in a closed reaction vessel to obtain a crystallized product; (3) calcining the crystallized product to remove the template and obtain the molecular sieve.
4. The preparation method according to claim 3, characterized in that: The organic template is 4-pyrrolidinopyridine.
5. The preparation method according to claim 3, characterized in that: The phosphorus source is selected from phosphoric acid and / or phosphorus pentoxide; The aluminum source is selected from at least one of pseudo-boehmite, aluminum hydroxide or aluminum isopropoxide; The silicon source is selected from at least one of silica sol, ethyl orthosilicate, tetramethoxysilane or white carbon black; The mineralizer is selected from HF and / or NH4F; The solvent is selected from alcohols.
6. The preparation method according to claim 3, characterized in that The alcohol is selected from at least one of cyclohexanol, ethylene glycol, diethylene glycol and triethylene glycol.
7. The preparation method according to claim 3, characterized in that: The molar composition of the mixture is aR: bHF: cH3PO4: qSiO2: Al2O3: mROH: nH2O; in, a=0.1~5.0; b=1.0~5.0; c=0.5~5.0; q=0~1.0; m=0~100; n=5~100。 8. The preparation method according to claim 3, characterized in that: The crystallization temperature is 130-200°C; The crystallization time is 1 to 15 days.
9. The preparation method according to claim 3, characterized in that: The crystallization temperature is 150-200°C.
10. Use of the molecular sieve according to any one of claims 1 or 2, characterized in that: As water adsorbent.
Citation Information
Patent Citations
Method for synthesizing silicoaluminophosphate molecular sieve SAPO-11 at normal pressure
CN102786063A
Silicon-aluminum phosphate molecular sieve with ATS skeleton structure, as well as preparation method and application thereof
CN110817898A
AFN structure silicon-phosphorus-aluminum molecular sieve as well as synthesis method and application thereof
CN112079363A
Preparation method and application of DDR molecular sieve
CN114516639A
Synthetic process of SAPO-11 Molecular sieve
CN1834015A