Preparation method of composite electrode material with porous honeycomb structure

By using a composite electrode material with a porous honeycomb structure in sodium ion battery electrode material and combining a single atomic catalyst, the reversible dynamic conversion and dissolution loss of transition metal chalcogenide electrode material is solved, which significantly improves the cycle life and reversibility of the battery capacity.

CN118929772APending Publication Date: 2024-11-12YANGTZE NORMAL UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410918866.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Transition metal chalcogenide electrode materials have problems such as poor reversible dynamic conversion reaction, loss of sodium polysulfide (selenium) sodium, slow ion transfer rate and serious volume expansion in sodium ion batteries.

Method used

Using a composite electrode material with a porous honeycomb structure, it is prepared by loading particulate transition metal chalcogenides on ultra-thin carbon nanosheets and evenly distributing single atomic catalyst on its surface, and is prepared by high-temperature carbonization and sulfur (selenium) treatment to form TMC/SAM'@NC composites.

Benefits of technology

It improves the cycle life and reversible capacity of the electrode material, reduces the dissolution loss of NaPSs, promotes efficient reversible catalytic conversion of M and Na2S, solves the problems of slow ion transmission rate and volume expansion, and significantly improves the performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004936011920000011
    Figure HDA0004936011920000011
  • Figure HDA0004936011920000012
    Figure HDA0004936011920000012
  • Figure HDA0004936011920000021
    Figure HDA0004936011920000021
Patent Text Reader

Abstract

The invention discloses a preparation method of a composite electrode material with a porous honeycomb structure, the electrode material comprises a porous honeycomb structure constructed by metal monatomic doped ultrathin carbon nanosheets, and granular transition metal chalcogenide is also loaded on the carbon nanosheets; the chemical general formula of the electrode material is TMC / SAM '(at) NC. The carbon-supported monatomic catalyst in the structure can provide abundant active metal active sites, high conductivity and strong chemical adsorption / conversion capacity of M '-N bonds in the charging and discharging process of TMC, and can also immobilize NaPSs (NaPSes), so that the problem of poor reversible dynamic conversion of M / Na2S in the sodium storage process of TMC is solved, and the preparation method is simple and easy to implement. And the TMC nanoparticles are uniformly anchored on the three-dimensional honeycomb carbon structure, so that the volume expansion of the TMCs in the cycle process is relieved, and the cycle stability and reversible capacity of the TMC are remarkably improved. The preparation method is low in raw material cost, simple in process, easy in realization of reaction conditions, capable of realizing batch production and convenient for commercialized application, and has a huge application prospect in sodium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion battery materials, and in particular relates to a method for preparing a composite electrode material with a porous honeycomb structure. Background Art

[0002] The pursuit of carbon neutrality has created a huge demand for large-watt-hour-scale batteries, which in turn has promoted the rapid development of energy storage technology. Over the past few decades, lithium-ion batteries have been widely studied due to their high energy density. Although lithium-ion batteries have revolutionized our lifestyle due to their perfect combination of high energy density and long cycle life, they cannot meet the growing demand for large-scale energy storage due to the high cost caused by limited lithium resources. In contrast, sodium-ion batteries made from abundant sodium resources have high compatibility with aluminum current collectors, which may reduce manufacturing costs. In addition, sodium is the lightest and smallest element among alkali metals after lithium, and is expected to perform as well as lithium-ion technology. Given the above characteristics, as the world is transitioning to renewable energy, sodium-ion batteries (SIBs) may be the answer to our search for cost-effective and sustainable alternatives in large-scale energy storage.

[0003] Anode materials are one of the key components for building high-performance SIBs, which determines the energy density and operating voltage window of the battery. In recent years, a series of materials such as carbon materials, alloy materials, metal phosphides, metal oxides, metal sulfides and metal selenides have been studied as potential anode materials for SIBs. Carbonaceous materials have excellent long-term cycling stability, but their low reversible capacity limits their application in high energy density sodium-ion batteries. Alloy materials are prone to rapid capacity decay due to the huge volume change during the sodium / desodium process, which leads to the rupture of active materials. Although metal phosphides claim to provide high theoretical capacity, the use of hazardous precursors and their poor electronic conductivity limit their practicality in certain applications. Among various anode materials, transition metal chalcogenides (TMCs) have attracted widespread attention due to their advantages such as large theoretical capacity, good cycling stability, easy structure control and adjustable chemical composition. Unfortunately, there are still many challenges in the application of transition metal chalcogenides in SIBs, such as poor conductivity. 、 Large volume changes, unclear sodium storage mechanism, etc. More importantly, the electronic conductivity of TMC discharge products (such as Na2S, Na2Se, etc.) is extremely poor. During the charging process, they will irreversibly transform into M and Na2S / Na2Se instead of the original TMC, which will cause S or Se to replace TMC as active materials for sodium storage after the first cycle. Ultimately, this mechanism leads to the dissolution and loss of TMC during the charge and discharge process, resulting in low utilization of TMC active materials, passivation of the sodium electrode surface, and increased interface resistance.

[0004] Studies have found that reasonable nanostructure engineering can significantly improve the phase stability and electrochemical sodium storage capacity of TMC, such as designing special nanostructured TMC solid solutions to improve reaction kinetics and maintain structural stability, or constructing heterogeneous interface engineering to improve conductivity and promote ion transfer kinetics. Based on this idea, researchers have proposed many improved technical solutions such as nano-sizing transition metal sulfide negative electrode materials, preparing transition metal sulfide negative electrode materials into special structures, and modifying transition metal sulfides with carbon materials. For example, the invention patent CN110048106A discloses a cobalt sulfide and multi-level carbon nanostructure composite material and its preparation method and application. With nitrogen-sulfur co-doped graphene as the matrix, the method of metal catalysis to generate carbon nanotubes is used to grow carbon nanotubes in situ on graphene, and cobalt particles are wrapped in the tubes. After that, the cobalt particles are sulfurized to generate a material composite of cobalt sulfide and multi-level carbon structure. The invention patent CN112850690A discloses a preparation method and sodium storage application of a graphene-loaded double transition metal sulfide composite material. The method comprises: preparing a graphene-loaded intercalated cobalt-aluminum hydrotalcite precursor using graphene, ammonium molybdate, cobalt nitrate, aluminum nitrate and sodium hydroxide as raw materials, hydrothermal vulcanization, calcination to improve crystallinity, and obtaining a Co9S8@MoS2 ring nanocomposite material loaded with reduced graphene oxide. Invention patent CN109935815A discloses a carbon-coated polysulfide heterojunction material, which is composed of a core body and a shell coated on the outside of the core body, wherein the core body is a polysulfide heterojunction and the shell is a carbon layer. Although the above method can slow down the huge volume change produced in the electrochemical process and improve the conductivity and cycle stability to a certain extent, the problems related to the poor reversible dynamic conversion reaction of metal sulfide electrode materials, material separation and sodium polysulfide shuttling still occur.

[0005] Single-atom catalysts (SACs) refer to metal particles with catalytic active centers that are reduced to atomic scale, and the metal is uniformly distributed on the carrier in the form of single atoms. It has been proved through theory and experiment that the functionalization and doping of transition metal single atoms (Single atomic metal, SAM', M'=Fe, Co, Ni, Mn, V, Zn, Cu, etc.) catalysts with uniform active center sites and high atomic utilization on nitrogen-rich carbonaceous materials (SAM'-NC) is beneficial to improve conductivity, enhance adsorption energy and catalytic activity. In addition, carbon-supported SAM' can not only reduce transfer resistance and promote the affinity of sodium ions in carbon materials, but also have low cost, variable selectivity and considerable intrinsic activity, all of which improve the performance of the battery. In this case, if carbon-supported SAM' is used, it may accelerate the formation and decomposition of lithium / sodium polysulfides in Li / Na-S batteries. Remarkable results have been achieved. Therefore, carbon-supported SAM' catalysts are also expected to achieve good results in enhancing the dynamic characteristics of TMC and reversible phase transitions during the cycle process. It is worth noting that nanostructure regulation is often the key to controlling electrode performance, and the synthesis of a certain nanostructure is conducive to promoting the activation reaction. However, single-atom catalysts have abundant active sites and maximum atomic utilization, which makes their catalytic activity high. Due to the reduction in the size of nanoparticles, the surface energy of atoms increases, and they are easy to aggregate into clusters, resulting in reduced loading and performance. Therefore, it is still a huge challenge to explore the synthesis strategy of coupling transition metal chalcogenides with single-atom catalysts with uniform atomic active sites, easy exposure, and high stability, as well as to achieve excellent electrochemical performance. At present, few related reports focus on the functionalization of single-atom catalysts with TMCs to solve the problem of reversible dynamic transformation during the charging and discharging process of TMCs. Summary of the invention

[0006] In view of this, the purpose of the present invention is to provide a method for preparing a composite electrode material with a porous honeycomb structure, which solves the problems of poor reversible dynamic conversion reaction, dissolution and loss of sodium polysulfide (selenide), slow ion transfer rate and severe volume expansion in existing metal chalcogenide electrode materials.

[0007] To achieve the above object, the present invention provides the following technical solutions: a method for preparing a composite electrode material with a porous honeycomb structure, wherein the electrode material comprises a porous honeycomb structure constructed by ultrathin carbon nanosheets doped with metal single atoms, and the carbon nanosheets are also loaded with granular transition metal chalcogenides; the chemical formula of the electrode material is TMC / SAM'@NC, wherein TMC is a transition metal chalcogenide, M is a transition metal, M' is a single atom Fe, Co, Ni, Mn, V, Zn, Cu or Cr, and NC is a carbon nanosheet, wherein M and M' are independently selected and are different; the method for preparing the electrode material comprises the following steps:

[0008] 1) dissolving polyvinyl pyrrolidone in water and stirring evenly, then adding salts containing M and salts containing M', stirring continuously until completely dissolved, and drying the mixed solution to obtain a reddish brown solid powder; the concentration of the salt containing M in the mixed solution is 0.05-0.5M, and the concentration of the salt containing M' is 0.002-0.008M;

[0009] 2) The solid powder obtained in step 1) is transferred into a tube furnace and carbonized in a protective atmosphere. After the reaction is completed, the temperature is naturally lowered to obtain MC x / SAM'@NC or M / SAM'@NC composites;

[0010] 3) MC prepared in step 2) x / SAM'@NC or M / SAM'@NC and a sulfur source or a selenium source are placed in two porcelain boats respectively and wrapped with a piece of tin foil, and then subjected to sulfurization or selenization treatment in a protective atmosphere. After the reaction is completed, the temperature is naturally lowered to prepare the TMC / SAM'@NC composite electrode material.

[0011] Preferably, the polyvinyl pyrrolidone is one or more of K23-27, K29-32, K30 and K88-96.

[0012] Preferably, the salt in step 1) is one or more of nitrate, acetate and chloride.

[0013] Preferably, the concentration of polyvinyl pyrrolidone in the mixed solution is 0.05-0.15 g / ml; and the drying temperature is 50-90°C.

[0014] Preferably, the sulfur source is thiourea or sulfur powder; the selenium source is selenium powder or sodium selenite; the MC x The mass ratio of M / SAM'@NC or M / SAM'@NC to the sulfur source or selenium source is 1:1 to 1:5.

[0015] Preferably, the carbonization treatment is performed by heating the temperature to 150-300°C at a heating rate of 1-10°C / min and keeping the temperature for 0.5-6h, then heating the temperature to 600-1000°C at a heating rate of 1-10°C / min and keeping the temperature for 0.5-6h.

[0016] Preferably, the sulfidation / selenization treatment is carried out by heating the temperature to 400-600° C. at a heating rate of 1-10° C. / min and maintaining the temperature for 0.5-5 h.

[0017] Preferably, the protective atmosphere is argon or nitrogen.

[0018] Another object of the present invention is to provide a composite electrode material with a porous honeycomb structure prepared by the above method.

[0019] Another object of the present invention is to provide an application of the above composite electrode material in a sodium ion battery.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. The present invention provides a method for preparing a composite electrode material with a porous honeycomb structure, using transition metal chalcogenides coupled with carbon-supported single-atom catalysts, so that a large number of metal chalcogenide nanoparticles are uniformly attached to the surface of carbon-supported single-atom nanosheets with a porous honeycomb structure, and the single atoms and metal sulfides are uniformly dispersed, without agglomeration, and have a high loading capacity. Among them, the carbon-supported single-atom catalyst can provide abundant active metal active sites, high conductivity and strong chemical adsorption / conversion ability of M'-N bonds during the TMC charging and discharging process, and can also immobilize NaPSs (NaPSes), thereby reducing the dissolution loss of NaPSs (NaPSes), and promoting the efficient reversible catalytic conversion of M and Na2S (Na2Se) to the parent TMC, so that TMC exhibits excellent cycle life and ultra-high reversible capacity, thereby solving the problem of poor reversible dynamic conversion of M / Na2S and dissolution loss of polysulfides in the sodium storage process of TMC, and also solving the problem of slow ion transmission rate and severe volume expansion of metal chalcogenide electrode materials, showing excellent application prospects in the field of sodium ions.

[0022] 2. The composite electrode material prepared by the present invention has a unique three-dimensional honeycomb porous structure, which not only has excellent electrical conductivity and but also exhibits a large specific surface area, thereby greatly shortening the diffusion path of sodium ions / electrons, while providing abundant sodium ion storage sites and a large direct contact area between the electrode and the electrolyte. Secondly, the TMC nanoparticles are evenly anchored on the three-dimensional honeycomb carbon structure to alleviate the volume expansion of TMC during the cycle. Not only that, the present invention dopes the carbon-rich material with a transition metal single atom catalyst, which can further improve the conductivity and electrochemical properties of the carbon skeleton. More importantly, the transition metal single atom catalyst can also enhance the affinity of sodium ions in carbonaceous materials and reduce the transfer resistance of sodium ions. The electrode material of the present invention is 20Ag -1 The cycle life of more than 2200 cycles was shown at a current density of 405.9 mAh g -1 Therefore, the porous honeycomb transition metal chalcogenide coupled carbon-supported single-atom catalyst electrode material formed by the present invention exhibits excellent cycle life, high reversible capacity and excellent rate capability, providing a new idea and theoretical basis for the improvement of transition metal chalcogenide electrode materials.

[0023] 3. The present invention uses polyvinyl pyrrolidone as the main raw material, and can simultaneously realize the doping of transition metal single atoms and the loading of metal chalcogenides through simple high-temperature carbonization, sulfur (selenization) treatment and other means. The operation is simple, and the cost of raw materials is low, the process is simple, the energy consumption is low, and the reaction conditions are easier to achieve. It can be mass-produced and is convenient for commercial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the scanning electron microscope image of FeC3 / SAMn@NC prepared in Example 1.

[0025] Figure 2 Scanning electron microscopy (ac), transmission electron microscopy (d~e) and spherical aberration electron microscopy (f) of FeS2 / SAMn@NC prepared in Example 1.

[0026] Figure 3 This is the X-ray diffraction pattern of the FeS2 / SAMn@NC composite electrode material prepared in Example 1.

[0027] Figure 4 This is the thermogravimetric analysis diagram of the FeS2 / SAMn@NC composite electrode material prepared in Example 1.

[0028] Figure 5 This is the rate performance diagram of the FeS2 / SAMn@NC composite electrode material prepared in Example 1.

[0029] Figure 6The half-cell prepared for FeS2 / SAMn@NC electrode material was tested at 1.0Ag -1 Charge and discharge curves under current density (a) and cycle stability test (b).

[0030] Figure 7 The half-cell prepared for FeS2 / SAMn@NC electrode material is at 20.0A g -1 Cyclic voltammetry curves at different current densities. DETAILED DESCRIPTION

[0031] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, but the embodiments are not intended to limit the present invention. The experimental methods without specific conditions in the preferred embodiments are usually carried out under conventional conditions or under conditions recommended by the reagent manufacturer.

[0032] 1. A method for preparing a composite electrode material with a porous honeycomb structure

[0033] Example 1

[0034] 1) Dissolve 3 g of polyvinyl pyrrolidone with a molecular weight of 40,000 in 45 ml of deionized water and stir for 30 min. Then add 4.5 g of Fe(NO3)3·9H2O and 0.075 g of Mn(CH3COO)2·4H2O and continue stirring until they are completely dissolved. Then transfer the mixed solution into an oven and dry it at 60°C to obtain a reddish-brown solid powder.

[0035] 2) The solid powder obtained in step 1) was transferred into a tube furnace and heated at 5°C min -1 The temperature was raised to 200 °C at a heating rate of 5 °C min -1 The temperature was raised to 800°C at a heating rate and kept for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the FeC3 / SAMn@NC composite material.

[0036] 3) The FeC3 / SAMn@NC and sulfur powder prepared in step 2) were placed in two porcelain boats at a mass ratio of 1:5 and wrapped with a piece of tin foil. Then, the boats were heated at 2°C min under an argon atmosphere. -1 The temperature was raised to 500°C at a heating rate and kept for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the FeS2 / SAMn@NC composite electrode material.

[0037] Example 2

[0038] 1) Dissolve 3 g of polyvinyl pyrrolidone with a molecular weight of 58,000 in 45 ml of deionized water and stir for 30 min. Then add 4.5 g of Fe(NO3)3·9H2O and 0.075 g of Mn(CH3COO)2·4H2O and continue stirring until they are completely dissolved. Then transfer the mixed solution into an oven and dry it at 60°C to obtain a reddish-brown solid powder.

[0039] 2) The solid powder obtained in step 1) was transferred into a tube furnace and heated at 5°C min -1 The temperature was raised to 200 °C at a heating rate of 5 °C min -1 The temperature was raised to 800°C at a heating rate and kept for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the FeC3 / SAMn@NC composite material.

[0040] 3) The FeC3 / SAMn@NC and sulfur powder prepared in step 2) were placed in two porcelain boats at a mass ratio of 1:5 and wrapped with a piece of tin foil. Then, the boats were heated at 2°C min under an argon atmosphere. -1 The temperature was raised to 500°C at a heating rate and kept for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the FeS2 / SAMn@NC composite electrode material.

[0041] Example 3

[0042] 1) Dissolve 3 g of polyvinyl pyrrolidone with a molecular weight of 40,000 in 45 ml of deionized water and stir for 30 min. Then add 4.5 g of FeCl3·6H2O and 0.075 g of Mn(NO3)2·4H2O and continue stirring until they are completely dissolved. Then transfer the mixed solution into an oven and dry it at 60°C to obtain a reddish-brown solid powder.

[0043] 2) The solid powder obtained in step 1) was transferred into a tube furnace and heated at 5°C min -1 The temperature was raised to 200 °C at a heating rate of 5 °C min -1 The temperature was raised to 800°C at a heating rate and kept for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the FeC3 / SAMn@NC composite material.

[0044] 3) The FeC3 / SAMn@NC and sulfur powder prepared in step 2) were placed in two porcelain boats at a mass ratio of 1:5 and wrapped with a piece of tin foil. Then, the boats were heated at 2°C min under an argon atmosphere. -1The temperature was raised to 500°C at a heating rate and kept for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the FeS2 / SAMn@NC composite electrode material.

[0045] Example 4

[0046] 1) Dissolve 3 g of polyvinyl pyrrolidone with a molecular weight of 40,000 in 45 ml of deionized water and stir for 30 min. Then add 4.5 g of Fe(NO3)3·9H2O and 0.054 g of Cu(CH3COO)2·4H2O and continue stirring until they are completely dissolved. Then transfer the mixed solution into an oven and dry it at 60°C to obtain a reddish-brown solid powder.

[0047] 2) The solid powder obtained in step 1) was transferred into a tube furnace and heated at 5°C min -1 The temperature was raised to 200 °C at a heating rate of 5 °C min -1 The temperature was raised to 800°C at a heating rate and kept for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the FeC3 / SACu@NC composite material.

[0048] 3) The FeC3 / SACu@NC and sulfur powder prepared in step 2) were placed in two porcelain boats at a mass ratio of 1:5 and wrapped with a piece of tin foil. Then, the boats were heated at 2°C min under an argon atmosphere. -1 The temperature was raised to 500°C at a heating rate and kept for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the FeS2 / SACu@NC composite electrode material.

[0049] Example 5

[0050] 1) Dissolve 3 g of polyvinyl pyrrolidone with a molecular weight of 40,000 in 45 ml of deionized water and stir for 30 min. Then add 3.2 g of Co(NO3)3·6H2O and 0.075 g of Mn(CH3COO)2·4H2O and continue stirring until completely dissolved. Then transfer the mixed solution into an oven and dry it at 60°C to obtain a reddish-brown solid powder.

[0051] 2) The solid powder obtained in step 1) was transferred into a tube furnace and heated at 5°C min -1 The temperature was raised to 200 °C at a heating rate of 5 °C min -1 The temperature was raised to 800°C at a heating rate and kept for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the Co / SAMn@NC composite material.

[0052] 3) The Co / SAMn@NC and sulfur powder prepared in step 2) were placed in two porcelain boats at a mass ratio of 1:5 and wrapped with a piece of tin foil. Then, the boats were placed in an argon atmosphere at 2°C min -1 The temperature was raised to 500°C at a heating rate and kept for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the CoS2 / SAMn@NC composite electrode material.

[0053] Example 6

[0054] 1) Dissolve 3 g of polyvinyl pyrrolidone with a molecular weight of 40,000 in 45 ml of deionized water and stir for 30 min. Then add 3.2 g of Co(NO3)3·6H2O and 0.054 g of Cu(CH3COO)2·4H2O and continue stirring until completely dissolved. Then transfer the mixed solution into an oven and dry it at 60°C to obtain a reddish-brown solid powder.

[0055] 2) The solid powder obtained in step 1) was transferred into a tube furnace and heated at 5°C min -1 The temperature was raised to 200 °C at a heating rate of 5 °C min -1 The temperature was raised to 800°C at a heating rate and kept for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the Co / SACu@NC composite material.

[0056] 3) The Co / SACu@NC and sulfur powder prepared in step 2) were placed in two porcelain boats at a mass ratio of 1:5 and wrapped with a piece of tin foil. The boats were then placed in an argon atmosphere at 2°C min -1 The temperature was raised to 500°C at a heating rate and kept for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the CoS2 / SACu@NC composite electrode material.

[0057] 2. Performance Testing

[0058] 1. The morphology of the FeC3 / SAMn@NC and FeS2 / SAMn@NC composite materials prepared in Example 1 was observed under a scanning microscope and a transmission electron microscope. The results are as follows: Figure 1 and Figure 2 shown.

[0059] Depend on Figure 1 a It can be seen that the intermediate product FeC3 / SAMn@NC exhibits a porous honeycomb structure. Figure 1 b and Figure 1 c shows that the porous honeycomb structure is composed of ultra-thin carbon-supported Mn single-atom nanosheets, and the surface of the nanosheets is very smooth and flat. Figure 2From a to c, we can see that FeS2 / SAMn@NC obtained after high-temperature sulfurization of FeC3 / SAMn@NC maintains a good porous honeycomb structure, but a large number of FeS2 nanoparticles are evenly attached to the surface of the carbon nanosheets. Figure 2 From the transmission electron microscopy images d to e, we can see that a large number of FeS2 nanoparticles are attached to the surface of the ultra-thin carbon nanosheets. Figure 2 From the spherical aberration electron microscope image of f, it can be seen that a large number of Mn single atoms are evenly dispersed on the carbon nanosheets.

[0060] 2. The FeS2 / SAMn@NC composite electrode material prepared in Example 1 was subjected to X-ray diffraction and thermogravimetric analysis, and the results were as follows: Figure 3 and Figure 4 shown.

[0061] from Figure 3 From the X-ray diffraction pattern, we can see that the FeS2 / SAMn@NC composite material is mainly composed of cubic FeS2, and a relatively obvious diffraction peak appears at around 26°, proving that the carbon nanosheets have good crystallinity. Figure 4 From the thermogravimetric analysis diagram, it can be seen that there is a slight mass loss from room temperature to 200°C, which is mainly caused by the volatilization of the attached water inside the sample. The mass increase from 200°C to 500°C is due to the reaction of FeS2 with oxygen in the air to generate Fe2(SO4)3, and the mass loss from 500°C to 800°C is due to the production of SO2, SeO2 and CO2 gases. The final stability at 800°C is due to the production of Fe2O3 and Mn2O3. Through analysis, the mass percentage of FeS2 in the composite material is about 78.4%.

[0062] 3. Take the FeS2 / SAMn@NC composite material prepared in Example 1 as the negative electrode material and mix it with Ketjen black and CMC binder in a mass percentage of 70:20:10, then add an appropriate amount of deionized water, grind it in an agate mortar to a paste, apply it on a copper foil with a diameter of 13 mm, and then vacuum dry the copper foil at 80°C for 12 hours to obtain the negative electrode sheet of the sodium ion battery, and then transfer it to a glove box filled with argon gas for assembly of button batteries. The button battery model is CR2032, the metal sodium sheet is used as the counter electrode, the diaphragm is glass fiber, and the electrolyte is 1 mol / L NaCF3SO3 solution (the solvent is diethylene glycol dimethyl ether solution). The CR2032 button batteries assembled with FeS2 / SAMn@NC electrode materials are respectively 0.2~20.0Ag -1 The discharge capacity was measured under the current density condition (on Land 2001A test system, the voltage range was 0.01~3.0V, the same below), and the results were as follows Figure 5 shown.

[0063] It can be seen from the figure that when the current density is 0.2, 0.5, 1.0, 2.0, 5.0, 10.0 and 20.0A g -1 When the discharge capacities are 749.0, 719.5, 684.8, 648.3, 600.3, 544.2 and 459.5 mAh g -1 When the current density quickly returns to the initial value of 0.2A g -1 Its specific capacity is 689.8 mAh g -1 , and its capacity retention rate is 92.1%, indicating that the FeS2 / SAMn@NC composite material has excellent rate performance.

[0064] 4. The CR2032 button cell assembled with FeS2 / SAMn@NC electrode material was heated to 1.0A g -1 The cycle stability test was carried out at a current density of Figure 6 shown.

[0065] from Figure 6 As can be seen from a, the initial charge and discharge capacities of the FeS2 / SAMn@NC electrode materials prepared in the present invention are 782.9 mAh g -1 and 854.8mAh g -1 , the corresponding initial coulombic efficiency is 91.6%, and from the second to the third cycle, the charge and discharge curves of FeS2 / SAMn@NC almost overlap and the coulombic efficiency remains at 100%, indicating that FeS2 / SAMn@NC has good cycle stability. Figure 6 As can be seen in b, after the electrode has been cycled 80 times, its discharge capacity is still 658.5 mAh g -1 , the capacity retention is 77.1% of the initial discharge capacity, indicating that the material has a large specific capacity and good cycle stability.

[0066] 5. The CR2032 button cell assembled with FeS2 / SAMn@NC electrode material was heated to 20.0A g -1 The cycle stability test was carried out at a current density of Figure 7 shown.

[0067] It can be seen from the figure that the FeS2 / SAMn@NC electrode material prepared by the present invention has good conductivity even at 20.0A g -1 At a current density of 1.34 W, the initial charge and discharge capacities were 462.1 mAh g -1 and 521.9mAh g -1 After 2200 cycles, its discharge capacity is still 405.9 mAh g -1The capacity retention rate is 84% ​​of the initial discharge capacity, and the average capacity decay rate per cycle is only 0.05%, indicating that the FeS2 / SAMn@NC electrode material still has good structural stability and cycle life at ultra-high current density.

[0068] It should be noted that the electrode materials prepared in Examples 2 to 6 also have good and cycle-stable electrochemical properties, which are not listed here one by one.

[0069] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A method for preparing a composite electrode material with a porous honeycomb structure, characterized in that: The electrode material comprises a porous honeycomb structure constructed by ultrathin carbon nanosheets doped with metal single atoms, and the carbon nanosheets are also loaded with granular transition metal chalcogenides; the chemical formula of the electrode material is TMC / SAM'@NC, wherein TMC is a transition metal chalcogenide, M is a transition metal, M' is a single atom Fe, Co, Ni, Mn, V, Zn, Cu or Cr, NC is a carbon nanosheet, and M and M' are independently selected and different; the preparation method of the electrode material comprises the following steps: 1) dissolving polyvinyl pyrrolidone in water and stirring evenly, then adding salts containing M and salts containing M', stirring continuously until completely dissolved, and drying the mixed solution to obtain a reddish brown solid powder; the concentration of the salt containing M in the mixed solution is 0.05-0.5M, and the concentration of the salt containing M' is 0.002-0.008M; 2) The solid powder obtained in step 1) is transferred into a tube furnace and carbonized in a protective atmosphere. After the reaction is completed, the temperature is naturally lowered to obtain MC x / SAM'@NC or M / SAM'@NC composites; 3) MC prepared in step 2) x / SAM'@NC or M / SAM'@NC and a sulfur source or a selenium source are placed in two porcelain boats respectively and wrapped with a piece of tin foil, and then subjected to sulfurization or selenization treatment in a protective atmosphere. After the reaction is completed, the temperature is naturally lowered to prepare the TMC / SAM'@NC composite electrode material.

2. The method for preparing the composite electrode material with a porous honeycomb structure according to claim 1, characterized in that: The polyvinyl pyrrolidone is one or more of K23-27, K29-32, K30 and K88-96.

3. The method for preparing the composite electrode material with a porous honeycomb structure according to claim 1, characterized in that: The salt in step 1) is one or more of nitrate, acetate and chloride.

4. The method for preparing the composite electrode material with a porous honeycomb structure according to claim 1, characterized in that: The concentration of polyvinyl pyrrolidone in the mixed solution is 0.05-0.15 g / ml; the drying temperature is 50-90°C.

5. The method for preparing the composite electrode material with a porous honeycomb structure according to claim 1, characterized in that: The sulfur source is thiourea or sulfur powder; the selenium source is selenium powder or sodium selenite; the MC x The mass ratio of M / SAM'@NC or M / SAM'@NC to the sulfur source / selenium source is 1:1 to 1:

5.

6. The method for preparing the composite electrode material with a porous honeycomb structure according to claim 1, characterized in that: The carbonization treatment is performed by heating the temperature to 150-300° C. at a heating rate of 1-10° C. / min and keeping the temperature for 0.5-6 hours, then heating the temperature to 600-1000° C. at a heating rate of 1-10° C. / min and keeping the temperature for 0.5-6 hours.

7. The method for preparing the composite electrode material with a porous honeycomb structure according to claim 1, characterized in that: The sulfurization / selenization treatment is carried out by heating the temperature to 400-600° C. at a heating rate of 1-10° C. / min and maintaining the temperature for 0.5-5 hours.

8. The method for preparing the composite electrode material with a porous honeycomb structure according to claim 1, characterized in that: The protective atmosphere is argon or nitrogen.

9. A composite electrode material with a porous honeycomb structure prepared by the method according to any one of claims 1 to 8.

10. Use of the composite electrode material according to claim 9 in a sodium ion battery.

Citation Information

Patent Citations

  • Carbon-coated polysulfide heterojunction material, preparation method and application

    CN109935815A

  • Cobalt sulfide and multilevel carbon nanometer structure composite material and preparation method and application thereof

    CN110048106A

  • Preparation method and sodium storage application of graphene-loaded double transition metal sulfide composite material

    CN112850690A