Preparation method of NiMoO4 / MoO3 nanosheet and application of NiMoO4 / MoO3 nanosheet in detection of trimethylamine

By growing NiMoO4 nanoparticles on two-dimensional MoO3 nanosheets, NiMoO4/MoO3 heterostructure was constructed, and the problems of low response and poor selectivity of existing sensors were solved, and efficient and accurate trimethylamine detection was achieved, suitable for food safety and environmental monitoring. .

CN118929782APending Publication Date: 2024-11-12SHENYANG INSTITUTE OF CHEMICAL TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410874090.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing metal oxide semiconductor gas sensors have problems such as low response, poor selectivity and poor stability in detecting trimethylamine, making it difficult to achieve efficient and accurate detection.

Method used

NiMoO4 nanoparticles were grown on two-dimensional MoO3 nanosheets through a two-step solvothermal process route to construct NiMoO4/MoO3 heterostructures to prepare efficient trimethylamine gas sensors. The method includes calcining ammonium molybdate tetrahydrate to obtain a MoO3 precursor, then stirring in methanol and H2O2 and sonication, then heating in a polytetrafluoroethylene stainless steel autoclave, and finally calcining in a muffle furnace to obtain NiMoO4/MoO3 nanometers and coated on an alumina ceramic tube for use in the gas sensor.

Benefits of technology

It achieves high sensing response, excellent selectivity and significant long-term stability to trimethylamine gas, is suitable for industrial production, and is suitable for food safety and environmental monitoring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929782A_ABST
    Figure CN118929782A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a NiMoO4 / MoO3 nanosheet and application of the NiMoO4 / MoO3 nanosheet in trimethylamine detection, and relates to preparation and application of the NiMoO4 / MoO3 nanosheet. The NiMoO4 / MoO3 nanosheet is prepared through a simple and controllable two-step solvothermal method, the whole production process is low in raw material cost, the technology is simple, controllability is high, the preparation period is short, and the preparation method is suitable for industrial production. The prepared material is high in purity, good in crystallization and suitable for large-scale industrial production. The NiMoO4 / MoO3 nanosheet prepared by the invention has good selectivity when being used for detecting trimethylamine, is not influenced by interference gases such as acetone, ethanol and ammonia, has relatively high response, good response recovery speed and excellent long-term stability, is applied to preparation of a gas sensor for efficiently and accurately detecting trimethylamine, and has wide application prospect. The method has a wide application prospect in the fields of food safety monitoring and intelligent health.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a nanosheet and application of the nanosheet to a gas sensor for detecting trimethylamine, and in particular to a method for preparing a NiMoO4 / MoO3 nanosheet and application of the nanosheet to detect trimethylamine. Background Art

[0002] Trimethylamine (TMA) is an important air pollutant, and its foul odor mainly comes from automobile exhaust, food residues, and livestock-related activities. Long-term exposure to trimethylamine can cause corneal damage, skin damage, respiratory irritation, and may cause liver, nervous and other physiological system disorders after inhalation. The National Institute for Occupational Safety and Health recommends that the exposure time should not exceed 10 hours and 15 minutes when the trimethylamine concentration is 10ppm and 15ppm, respectively. In addition, trimethylamine has been recognized as an important biomarker for disease diagnosis and human health monitoring. For example, trimethylamine concentrations of more than 0.2ppm can be detected in the exhaled breath of patients with chronic kidney disease. In addition, trimethylamine is released during the degradation of seafood, and its concentration can be used as an evaluation indicator of freshness during seafood transportation. Therefore, the detection and measurement of trimethylamine levels are crucial in environmental monitoring, food safety, medical diagnosis, etc.

[0003] Metal oxide semiconductor (MOS) gas sensors have become widely used commercially due to their low cost and significant gas-sensing properties, but they still have disadvantages such as low response, poor selectivity, and poor stability. Therefore, it is essential to develop a sensitive, selective, and efficient trimethylamine sensor. Among them, MoO3, as a typical layered transition metal oxide, has attracted increasing interest due to its unique physical and chemical properties and can detect various gases. It is worth noting that the two-dimensional (2D) nanostructure has significant advantages, which promotes the diffusion of gas molecules over a large surface area and creates a wider electron depletion layer, facilitating the rapid detection of harmful gases. In addition, constructing a heterostructure by combining two different semiconductors can significantly affect various processes, including oxygen adsorption, catalytic activity, and charge transfer, thereby significantly enhancing the gas-sensing performance. Therefore, constructing a heterojunction involving 2D MoO3 nanomaterials and p-type or n-type MOS is a promising approach to overcome the limitations of sensors in detecting specific gases. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing NiMoO4 / MoO3 nanosheets and their trimethylamine detection application. The present invention grows NiMoO4 nanoparticles on two-dimensional MoO3 nanosheets through a two-step solvothermal process route to construct a carefully designed NiMoO4 / MoO3 heterostructure. It exhibits very high sensing response, excellent selectivity and significant long-term stability to trimethylamine gas, and its greatest advantage is that it can detect efficiently and accurately.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] A method for preparing NiMoO4 / MoO3 nanosheets, the specific process and steps of the method:

[0007] (1) Weigh ammonium molybdate tetrahydrate ((NH4)6Mo7O 24 ·4H2O), calcined at 500℃ for 2h to obtain MoO3 precursor;

[0008] (2) The MoO3 precursor prepared above was dissolved in H2O2 (30%) and stirred for 5 min, then methanol was added and stirred for 24 h, and ultrasonic treatment was performed at room temperature for 30 min, then the solution was transferred into a stainless steel high-pressure reactor lined with polytetrafluoroethylene, placed in an oven and heated to 180°C for 12 h, and the powder was collected after natural cooling, and washed with deionized water and ethanol by centrifugation for 3 times, and then kept at 60°C for drying for use; the precursor was directly placed in a muffle furnace and heated to 400°C for 2 h to obtain pure MoO3 nanosheet material;

[0009] (3) The MoO3 nanosheets obtained above were dispersed in ethanol and ultrasonically treated for 1 h. Then nickel nitrate hexahydrate (Ni(NO3)2·6H2O) and hexamethylenetetramine (C6H 12 N4), stirred for 30 min. The obtained mixture was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene and heated at 120°C for 4 h. After cooling to room temperature, it was washed several times with deionized water and ethanol, and then dried at 60°C for 12 h.

[0010] (4) The dried product was placed in a clean crucible in a muffle furnace and calcined at 500° C. for 2 h to obtain NiMoO4 / MoO3 nanosheets, which were then stored in a desiccator for analysis and testing.

[0011] An application of NiMoO4 / MoO3 nanosheets to trimethylamine detection, wherein the NiMoO4 / MoO3 nanosheet material is used as a gas sensitive material to make a gas sensor for trimethylamine gas detection, and has the following process and steps:

[0012] (1) NiMoO4 / MoO3 nanosheets and anhydrous ethanol are mixed and ground to form a uniform coating, which is then coated on the outer wall of an Al2O3 alumina ceramic tube;

[0013] (2) Passing a nickel-chromium alloy heating wire through an Al2O3 alumina ceramic tube to adjust the test temperature;

[0014] (3) The four conductive wires of the ceramic tube and the two ends of the heating wire are welded to the six-pin base to obtain a gas sensor element; the gas sensitivity characteristics of the sensor are tested using a WS-30A gas sensitive tester at a test temperature of 100 to 350°C.

[0015] Advantages and beneficial effects of the present invention:

[0016] 1. The present invention grows NiMoO4 nanoparticles on two-dimensional MoO3 nanosheets through a two-step solvent thermal process route, and constructs a well-designed NiMoO4 / MoO3 heterostructure. The entire production process has low raw material cost, simple process, high controllability, and short preparation cycle. The prepared material has high purity, good crystallization, and is suitable for large-scale industrial production. It also shows very high sensing response, excellent selectivity, and significant long-term stability to trimethylamine gas. The biggest advantage is that it can be detected efficiently and accurately, which will provide a simple and fast technical means for accurately detecting complex environments and online monitoring of air pollutants.

[0017] 2. The present invention uses (NH4)6Mo7O 24 ·4H2O, Ni(NO3)2·6H2O and C6H 12 N4 was used as raw material, and NiMoO4 nanoparticles were grown on two-dimensional MoO3 nanosheets by a two-step solvothermal method to construct a carefully designed NiMoO4 / MoO3 heterostructure. On the one hand, NiMoO4 / MoO3 has a large specific surface area, which is conducive to the effective adsorption of gas molecules on the material surface; on the other hand, a pn heterojunction is formed at the NiMoO4 / MoO3 interface, which effectively regulates the interface potential, thereby giving the sensor higher sensing performance.

[0018] 3. The NiMoO4 / MoO3 nanosheet gas sensor produced by the present invention has a simple production process and low cost, is suitable for industrial mass production, and shows broad application prospects in the fields of food safety monitoring and smart health. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 XRD patterns of materials obtained for Examples 1-4;

[0020] Figure 2FE-SEM images of the materials obtained in Examples 1-4, (a) MoO3, (b) 5%-NiMoO4 / MoO3, (c) 7%-NiMoO4 / MoO3, (d) 10%-NiMoO4 / MoO3

[0021] Figure 3 Schematic diagram of the structure of the trimethylamine sensor;

[0022] Figure 4 It is the sensitivity of the gas sensor to 10ppm trimethylamine gas at a test temperature of 100-350℃;

[0023] Figure 5 The relationship curve between the response of the gas sensor at 200°C and the concentration of trimethylamine (0.1-1000ppm);

[0024] Figure 6 The selectivity of the gas sensor to 10 ppm gas at 200°C;

[0025] Figure 7 This is the response recovery curve of the gas sensor of Example 3 to 10 ppm trimethylamine gas at 200° C.;

[0026] Figure 8 This is the repeatability curve of the gas sensor of Example 3 at 200° C. for 10 ppm trimethylamine gas;

[0027] Fig. 9 The response of the gas sensor of Example 3 to 10 ppm trimethylamine within 40 days;

[0028] Fig.10 This is a comparison diagram of the embodiments. DETAILED DESCRIPTION

[0029] The present invention will be described in detail below with reference to the embodiments shown in the accompanying drawings.

[0030] The method for preparing NiMoO4MoO3 nanosheets comprises the following steps:

[0031] Example 1

[0032] Preparation of MoO3 nanosheets

[0033] Step 1: Weigh 10.00g (NH4)6Mo7O 24 4H2O, calcined at 500℃ for 2h to obtain MoO3 precursor;

[0034] Step 2: Weigh 0.72 g of the MoO3 precursor obtained in step 1 and dissolve it in H2O2 (30%) and stir for 5 min, then add methanol and stir for 24 h, and then ultrasonicate at room temperature for 30 min;

[0035] Step 3: Transfer the solution from step 2 to a stainless steel autoclave lined with polytetrafluoroethylene, place it in an oven and heat it to 180°C for 12 hours, and collect the powder after the temperature drops naturally;

[0036] Step 4: The powder collected in step 3 is washed by centrifugation with deionized water and ethanol for three times, and then dried at 60°C for later use;

[0037] Step 5: Place the precursor in step 4 directly into a muffle furnace and heat it to 400°C and keep it for 2 hours to obtain pure MoO3 nanosheet material.

[0038] Example 2

[0039] Preparation of 5%-NiMoO4 / MoO3 nanosheets

[0040] Steps 1, 2, 3, 4 and 5 are the same as in Example 1

[0041] Step 6: Disperse 0.0500 g of the MoO3 nanosheets obtained above in ethanol, ultrasonicate for 1 h, and then add 0.0051 g Ni(NO3)2·6H2O and 0.0404 g C6H 12 N4, stirred for 30 min. The resulting mixture was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene and heated at 120 °C for 4 h. After cooling to room temperature, it was washed several times with deionized water and ethanol, and then dried at 60 °C for 12 h.

[0042] Step 7: Place the dried product in a clean crucible in a muffle furnace and calcine at 500° C. for 2 h to obtain 5%-NiMoO4 / MoO3 nanosheets, which are then stored in a desiccator for analysis and testing.

[0043] Example 3

[0044] Preparation of 7%-NiMoO4 / MoO3 nanosheets

[0045] Steps 1, 2, 3, 4 and 5 are the same as in Example 1

[0046] Step 6: Disperse 0.0500 g of the MoO3 nanosheets obtained above in ethanol, ultrasonicate for 1 h, and then add 0.0071 g Ni(NO3)2·6H2O and 0.0566 g C6H 12 N4, stirred for 30 min. The resulting mixture was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene and heated at 120 °C for 4 h. After cooling to room temperature, it was washed several times with deionized water and ethanol, and then dried at 60 °C for 12 h.

[0047] Step 7: Place the dried product in a clean crucible and place it in a muffle furnace, calcine at 500° C. for 2 h to obtain 7%-NiMoO4 / MoO3 nanosheets, which are stored in a desiccator for analysis and detection.

[0048] Example 4

[0049] Preparation of 10%-NiMoO4 / MoO3 nanosheets

[0050] Steps 1, 2, 3, 4 and 5 are the same as in Example 1

[0051] Step 6: Disperse 0.0500 g of the MoO3 nanosheets obtained above in ethanol, ultrasonicate for 1 h, and then add 0.0101 g of Ni(NO3)2·6H2O and 0.0808 g of C6H 12 N4, stirred for 30 min. The resulting mixture was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene and heated at 120 °C for 4 h. After cooling to room temperature, it was washed several times with deionized water and ethanol, and then dried at 60 °C for 12 h.

[0052] Step 7: Place the dried product in a clean crucible and place it in a muffle furnace, calcine at 500° C. for 2 h to obtain 10%-NiMoO4 / MoO3 nanosheets, which are stored in a desiccator for analysis and detection.

[0053] Structural characterization of NiMoO4 / MoO3 composites

[0054] (1) XRD analysis

[0055] The XRD spectra of the materials obtained in Example 1-4 are as follows Figure 1 As shown. The diffraction peaks of the MoO3 sample correspond to α-MoO3 (JPCDS No. 35-0609). All diffraction peaks are clearly characterized, and no additional impurity diffraction peaks are observed, indicating that MoO3 has good crystallinity and high purity. The XRD spectrum of the NiMoO4 / MoO3 composite material is similar to that of pure MoO3, with a small amount of diffraction peaks belonging to NiMoO4 (JCPDS No. 31-0902). In addition, it is worth noting that with the increase in the introduction of nickel nitrate hexahydrate, the intensity of these characteristic peaks of NiMoO4 increases, confirming the successful formation of the NiMoO4 / MoO3 composite material.

[0056] (2) SEM analysis

[0057] The scanning electron microscope microstructure of the materials obtained in Examples 1-4 was analyzed. Figure 2As shown in the figure, the MoO3 sample presents a two-dimensional rectangular nanosheet structure with a smooth texture, extending for several microns and with a thickness ranging from 10 to 30 nm. These nanosheets are loosely stacked together to form more pores, which promote the rapid adsorption and desorption of gases during the gas sensing process. After the introduction of NiMoO4, NiMoO4 / MoO3 maintains the two-dimensional nanosheet structure and has a rougher texture compared to the original MoO3. The surface roughness is due to the secondary effective growth of NiMoO4 on the MoO3 surface.

[0058] (3) Gas-sensing performance test

[0059] Weigh a certain amount of NiMoO4 / MoO3 nanosheets and add anhydrous ethanol to make a slurry, which is then coated on an alumina ceramic tube. The alumina ceramic tube has two gold electrodes and four platinum wires, and a nickel-chromium heating wire in the tube. The ceramic tube is welded on a six-legged base, such as Figure 3 As shown, a gas sensor element is manufactured. Figure 4 The sensitivity curve of the gas sensor to 10ppm trimethylamine gas at different working temperatures (100-350℃) is shown in Figure 2. Figure 4 It can be clearly seen that within the test range, the sensitivity of several gas sensors varies, among which the best response value of the sensor in Example 1 is 12.54; the best response value of Example 2 is 52.16; the best response value of Example 3 is 62.92; and the best response value of Example 4 is 34.63. It can be clearly found that the sensor in Example 3 has more significant sensing characteristics. Figure 5 The sensing response to different concentrations of trimethylamine at 200°C is shown. In the concentration range of 0.1 to 50 ppm, the response values ​​of all sensors increase significantly with the increase of trimethylamine concentration. However, when the concentration of trimethylamine exceeds 50 ppm, the surface reaction decreases due to the extensive coverage of trimethylamine molecules on the surface of the sensing material, and the response increment tends to decrease. It is worth noting that the response value of the sensor in Example 3 is the highest; even at an extremely low concentration of 0.1 ppm, the sensor's response to trimethylamine is still large, reaching 3.98. This observation highlights its potential in detecting trace amounts of trimethylamine. Figure 6 The figure shows the selectivity test results of the sensor for various gases at 10ppm. It can be seen that the sensor is very sensitive to trimethylamine gas, while the response to other interfering gases (acetone, methanol, formaldehyde, ethanol, ammonia) is almost negligible, indicating that the sensor can selectively identify trimethylamine in organic volatile gases and has broad application prospects in the field of trimethylamine monitoring. Figure 7Shown is the response-recovery curve of the sensor of Example 3 to 10 ppm trimethylamine gas at an operating temperature of 200°C. It can be seen from the figure that the sensors experienced a rapid decline, stabilized in a stable state, and then recovered to their initial state when exposed to air. The response and recovery times were 13 and 78 s, respectively, indicating good response and recovery characteristics. Figure 8 It is shown that at an operating temperature of 200°C, Example 3 exhibits excellent reproducibility for 10 ppm trimethylamine, and Fig. 9 It can be seen that even after 40 days of testing, the sensor of Example 3 still exhibits good long-term stability.

Claims

1. A NiMoO 4 / MoO 3 Preparation method of nanosheets, It is characterized in that The specific process and steps of the method are as follows: (1) Weigh ammonium molybdate tetrahydrate (NH 4 ) 6 Mo 7 O 24 ·4H 2 O), calcined at 500 °C for 2 h to obtain MoO 3 Precursor; (2) Prepare MoO 3 The precursor is dissolved in H 2 O 2 (30%) was stirred for 5 min, methanol was added and stirred for 24 h, and ultrasonic treatment was performed at room temperature for 30 min. The solution was then transferred into a stainless steel autoclave lined with polytetrafluoroethylene, placed in an oven and heated to 180 °C for 12 h. The powder was collected after natural cooling, and washed with deionized water and ethanol by centrifugation for 3 times, and then kept at 60 °C for drying. The precursor was directly placed in a muffle furnace and heated to 400 °C for 2 h to obtain pure MoO 3 Nanosheet materials; (3) The MoO obtained above 3 The nanosheets were dispersed in ethanol and sonicated for 1 h, and then nickel nitrate hexahydrate (Ni(NO 3 ) 2 6H 2 O) and hexamethylenetetramine (C 6 H 12 N 4 ), stirred for 30 min. The resulting mixture was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene and heated at 120°C for 4 h. After cooling to room temperature, it was washed several times with deionized water and ethanol, and then dried at 60°C for 12 h; (4) The dried product was placed in a clean crucible and placed in a muffle furnace and calcined at 500 °C for 2 h to obtain NiMoO 4 / MoO 3 The nanosheets were stored in a desiccator until further analysis.

2. A NiMoO 4 / MoO 3 Application of nanosheets in the detection of trimethylamine, It is characterized in that The NiMoO 4 / MoO 3 Nanosheet materials are used as gas sensitive materials to make gas sensors for the detection of trimethylamine gas, with the following processes and steps: (1) NiMoO 4 / MoO 3 Nanosheets and anhydrous ethanol are mixed and ground into a uniform coating, which is then coated with Al 2 O 3 On the outer wall of alumina ceramic tube; (2) Pass the nickel-chromium alloy heating wire through the Al 2 O 3 Alumina ceramic tube to adjust the test temperature; (3) The four conductive wires of the ceramic tube and the two ends of the heating wire are welded to the six-pin base to obtain a gas sensor element; the gas sensitivity characteristics of the sensor are tested using a WS-30A gas sensitive tester at a test temperature of 100 to 350°C.