Composite electrode material for degrading chlorinated hydrocarbon pollutants as well as preparation method and application of composite electrode material

Preparation of Pd/Ni(OH)2/NF nickel-based composite electrode material by hydrothermal method and electrochemical deposition method, solving the efficiency and cost problems of traditional technology in trichloroethylene pollution treatment, and achieving high efficiency at room temperature and pressure The effect of degrading trichloroethylene and maintaining good catalytic activity and cycling performance over a wide pH range.

CN118929849APending Publication Date: 2024-11-12JIANGSU ENVIRONMENTAL ENG TECH CO LTD

Patent Information

Application Number
CN202410972401.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional chemical oxidation and in-situ thermal desorption have problems such as difficulty in controlling secondary pollution, difficulty in construction, and unsatisfactory results in treating trichloroethylene pollution. Moreover, the large-scale application cost of precious metal palladium is high, and nickel-based materials are in electricity. There are few studies on chemical hydrochloride.

Method used

The Pd/Ni(OH)2/NF nickel-based composite electrode material was prepared by hydrothermal method and electrochemical deposition. The electroactive sites of Pd nanoparticles were increased through the Ni(OH)2 nanoarray intermediate layer to form efficient and stable catalysis. Electrode material is used to hydrogenate and reduce trichloroethylene in an air atmosphere and at room temperature and pressure.

Benefits of technology

It has achieved rapid degradation of trichloroethylene, with fewer by-products, good catalytic activity and stability. It is suitable for the degradation of chlorinated hydrocarbon pollutants in groundwater, and remains highly efficient within a wide pH range and has excellent circulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929849A_ABST
    Figure CN118929849A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of reduction and repair of chlorinated hydrocarbon pollutants, in particular to a composite electrode material for degrading chlorinated hydrocarbon pollutants and a preparation method and application of the composite electrode material. Nickel nitrate hexahydrate, urea and ammonium fluoride are mixed to obtain a mixed solution, and the mixed solution and foamed nickel are subjected to a hydrothermal synthesis reaction; a foamed nickel substrate is coated with a Ni (OH) 2 nano array to obtain a Ni (OH) 2 / NF electrode material, then metal palladium is further electrically deposited, and the Pd / Ni (OH) 2 / NF nickel-based composite electrode material with the three-dimensional rose flower cluster morphology is prepared. The Pd / Ni (OH) 2 / NF nickel-based composite electrode material prepared by the invention is applied to air atmosphere, trichloroethylene is subjected to hydrogenation reduction at normal temperature and normal pressure, the reaction time is short, byproducts are few, and the Pd / Ni (OH) 2 / NF nickel-based composite electrode material has good activity and stability, and provides an effective way for degrading chlorinated hydrocarbon pollutants under actual underground water environment conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of reduction and restoration of chlorinated hydrocarbon pollutants, and in particular to a composite electrode material for degrading chlorinated hydrocarbon pollutants, and a preparation method and application thereof. Background Art

[0002] In recent years, trichloroethylene (TCE) has been found to be one of the most common industrial pollutants in groundwater. It has strong migration ability, long diffusion time, and uneven concentration distribution in aquifers. Traditional chemical oxidation, in-situ thermal desorption and other technologies have prominent problems such as difficulty in controlling secondary pollution, construction difficulties, and unsatisfactory results, posing great challenges to remediation.

[0003] Electrocatalytic hydrodechlorination (EHDC) is an emerging indirect electrochemical reduction technology that uses hydrogen radicals H, a strong reducing agent, to be generated on the cathode surface. * It undergoes rapid electrochemical reduction with chlorinated hydrocarbons, etc., and exhibits excellent dehalogenation and detoxification capabilities, with the advantages of controllable secondary pollution and low-carbon economy. Electrode materials are the core of electrocatalytic hydrogenation dechlorination technology, and their catalytic performance, stability, and cost-effectiveness are the most critical.

[0004] Various transition metals can catalyze H + Reduction to H * , such as Cu, Ni, Pd, Ag, etc., among which palladium-based (Pd) materials show the best catalytic activity because of its H * The generation and retention efficiency is the highest, which can adsorb H on the Pd surface. * (denoted as H * ads ), and can absorb H in the Pd lattice * (denoted as H * abs ) to form Pd hydride. However, how to reduce the high cost of large-scale application of precious metal Pd and improve its activity and efficiency in EHDC reaction is an urgent concern of researchers. At the same time, nickel-based (Ni) materials are low in cost and have similar H production properties as Pd. * Ability and stronger metal-hydrogen (MH * ) binding strength, and has been proven to have high activity and selectivity for enhancing EHDC. Among them, Ni(OH)2 is simple to synthesize, has a stable structure, and can effectively decompose water molecules to generate H * ,Currently, there is little research on electrochemical hydrodechlorination, which is mainly used in the field of supercapacitors.

[0005] Therefore, designing catalysts according to the dechlorination mechanism and achieving efficient dechlorination through the synergistic effect of multiple metals or metals and carriers has become one of the key research directions of this industry. Summary of the invention

[0006] The present invention aims at the above-mentioned technical problems, overcomes the shortcomings of the prior art, and provides a composite electrode material for degrading chlorinated hydrocarbon pollutants, and a preparation method and application thereof. The prepared Pd / Ni(OH)2 / NF nickel-based composite electrode material is used in an air atmosphere at room temperature and pressure to hydrogenate and reduce trichloroethylene. The reaction time is short, less by-products are produced, and the material has good activity and stability, and is suitable for the degradation of chlorinated hydrocarbon pollutants in groundwater.

[0007] In a first aspect, the present invention provides a method for preparing a composite electrode material for degrading chlorinated hydrocarbon pollutants, comprising the following steps:

[0008] Nickel nitrate hexahydrate (Ni(NO3) 2· 6H2O), urea (CO(NH2)2) and ammonium fluoride (NH4F), stirred at room temperature until clarified to obtain a mixed solution, wherein urea is a mild precipitant and ammonium fluoride is a morphology control agent, the mixed solution is subjected to a hydrothermal synthesis reaction with nickel foam, and a Ni(OH)2 nanoarray is coated on the nickel foam substrate to obtain a Ni(OH)2 / NF electrode material;

[0009] The Ni(OH)2 / NF electrode material is further electroplated with metal palladium to prepare a Pd / Ni(OH)2 / NF nickel-based composite electrode material with a three-dimensional rosette morphology.

[0010] Optionally, the molar ratio of the nickel nitrate hexahydrate, urea and ammonium fluoride is 1:4:2.

[0011] Optionally, the hydrothermal synthesis reaction specifically includes: placing the mixed solution and nickel foam in a polytetrafluoroethylene reactor liner, sealing it and placing it in an oven for heating reaction, washing the obtained sample with water and ethanol after cooling to room temperature, and obtaining a light green block Ni(OH)2 / NF electrode material with nickel foam as the base after drying.

[0012] Optionally, the nickel foam is pretreated before the hydrothermal synthesis reaction, specifically, the nickel foam is ultrasonically treated with hydrochloric acid, water, acetone and ethanol respectively, the ultrasonic treatment time is 15 to 30 minutes, the surface oxide layer and impurities such as grease are removed, the surface oxide layer and impurities such as grease are removed, and then the nickel foam is placed in an oven for drying and then left to stand for use.

[0013] Optionally, the hydrothermal synthesis reaction temperature is 160℃-200℃, the heating rate is 5℃ / min, and the reaction time is 4h-6h. The growth of Ni(OH)2 nanosheets is an anisotropic self-assembly mechanism, which can gradually grow into a compact rice ear layered structure under mild reaction temperature and sufficient reaction time.

[0014] Optionally, the specific steps of electro-depositing metal palladium include:

[0015] Preparation of electrolyte: palladium source and NaCl are mixed in water to prepare electrolyte, and ultrasonic treatment is performed until the palladium source is evenly dispersed and presents a brown-yellow clear solution;

[0016] Assembly of the reaction cell: Place the three-electrode system in a prepared electrolyte, wherein the Ni(OH)2 / NF electrode material is the working electrode, Pt is the counter electrode, and Ag / AgCl is the reference electrode. Electrodeposition is performed at a constant current of 7 mA and 313 K for 0.5-1 h, and the voltage is controlled at -0.8 V to prepare the Pd / Ni(OH)2 / NF nickel-based composite electrode material. The material can then be cleaned and dried with ultrapure water and anhydrous ethanol, respectively. The current density used for electrodeposition is a constant 7 mA, and the reaction time is preferably 0.5 to 1 h to avoid excessive growth and agglomeration of metal palladium.

[0017] It should be noted that in the assembly of the above reaction cell, a Pt sheet is used as the anode and nickel foam is used as the cathode, which are immersed in the above electrolyte. The Pd / NF electrode material obtained by constant current electrodeposition can be used as a reference group.

[0018] Optionally, the palladium source is at least one of palladium chloride and palladium nitrate.

[0019] Optionally, the drying temperature is lower than 80° C., and the drying method is vacuum drying or forced air drying, and vacuum drying is more preferred.

[0020] In a second aspect, the present invention provides a composite electrode material for degrading chlorinated hydrocarbon pollutants as a hydrogenation catalyst for degrading chlorinated hydrocarbon pollutants. The composite electrode material is prepared by the preparation method described in any one of the first aspects.

[0021] Optionally, in the composite electrode material, the loading amount of the active component palladium is 2.0 wt% to 3.0 wt% based on the mass of the metal palladium.

[0022] In a third aspect, the present invention further provides an application of the composite electrode material according to any scheme of the second aspect or the composite electrode material prepared by any preparation method of the first aspect as a catalyst in the hydrodechlorination degradation of chlorinated hydrocarbon pollutants.

[0023] Optionally, the chlorinated hydrocarbon pollutant includes trichloroethylene, which is used for trichloroethylene hydrodechlorination.

[0024] Optionally, a composite electrode material is used for the hydrodechlorination of trichloroethylene. The specific dechlorination reaction is carried out in a 100 mL electrochemical reaction cell, with an Ag / AgCl electrode as a reference electrode and a Pt sheet (2 cm×2 cm) as an anode, which are placed vertically and parallel to a Pd / Ni(OH)2 / NF electrode (2 cm×2 cm) with a spacing of 2 cm. The dechlorination experiment is carried out with trichloroethylene having an initial concentration of 20 mg / L, the electrolyte is 50 mM Na2SO4 solution, the reaction liquid volume is 80 mL, and an electrochemical workstation (Shanghai Chenhua, CHI760E) is used to control the constant potential electrolysis process and perform electrochemical analysis.

[0025] The electrochemical dechlorination reaction mechanism of chlorinated hydrocarbons described in the present invention (taking trichloroethylene as an example) is as follows: water is electrolyzed on the electron-rich Pd surface to produce a strong reducing agent, active hydrogen H * , where H * ads (adsorbed hydrogen) is accumulated on Pd NPs, which are rich in H * ads The environment is conducive to the rapid electrochemical reduction of TCE to form complete dechlorination products ethylene and ethane (Equations 1-3). Ethylene is usually further hydrogenated to ethane (Equation 4).

[0026] H2O + e - + Pd → Pd-H * ads + OH - (1)

[0027] C2HCl3 + 3H * ads +6e - → C2H4 + 3Cl - (2)

[0028] C2HCl3 + 5H * ads +8e - → C2H6 + 3Cl - (3)

[0029] C2H4 + 2H * ads → C2H6 (4)

[0030] The beneficial effects of the present invention are:

[0031] (1) The preparation method provided by the present invention combines the hydrothermal method and the electrochemical deposition method. The introduction of the Ni(OH)2 nanoarray intermediate layer can provide more electroactive sites for Pd nanoparticles under high current density conditions, thereby forming an efficient and stable catalytic electrode material;

[0032] (2) The preparation method provided by the present invention is simple and efficient, and can be easily industrialized and mass-produced. The electrode can maintain strong electrocatalytic activity in a wide pH range (pH = 3 to 9), and is not easily affected by common anions and cations in actual groundwater, demonstrating its feasibility for practical application in the degradation of trichloroethylene.

[0033] (3) The Pd / Ni(OH)2 / NF nickel-based composite electrode material prepared by the present invention is used for hydrogenation reduction of trichloroethylene in an air atmosphere at room temperature and pressure. The reaction time is short, the by-products are few, and the material has good activity and stability. After six cycles of use, the trichloroethylene removal rate is still maintained at more than 90%, and can reach up to 95%. The material has high reaction activity and good cycle performance, and provides an effective way to degrade chlorinated hydrocarbon pollutants under actual groundwater environmental conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Schematic diagram of the growth process of preparing electrode materials in Example 1 of the present invention;

[0035] Figure 2 XRD spectra of the electrode materials prepared in Example 1 and Comparative Examples 1-2 of the present invention;

[0036] Figure 3 middle, Figure 3 a and Figure 3 b are the GC-MS spectrum and GC spectrum during the reaction of Example 1 of the present invention, respectively; Figure 3 c is a diagram showing the dechlorination effect of Example 1 of the present invention;

[0037] Figure 4 The dechlorination effect diagram of the electrode materials prepared in Example 1 of the present invention and Comparative Examples 1-2 on 10 mg / L, 20 mg / L and 50 mg / L trichloroethylene;

[0038] Figure 5 It is a dechlorination effect diagram of Examples 7 to 16 of the present invention;

[0039] Figure 6 This is a diagram showing the dechlorination effect of Example 1 of the present invention in real groundwater;

[0040] Figure 7 The SEM comparison diagram of the electrode materials and the base material nickel foam prepared in Example 1 of the present invention and Comparative Examples 1-2;

[0041] Figure 8 TEM comparison diagram of Example 1 of the present invention and Comparative Example 1;

[0042] Fig. 9 middle, Fig. 9 a and Fig. 9b are the Pd 3d and Ni 2p XPS comparison spectra of Example 1 of the present invention and Comparative Example 1, respectively;

[0043] Fig.10 middle, Fig.10 a is the CV graph of the electrode material prepared in Example 1 with or without the addition of trichloroethylene, Fig.10 b is the CV comparison diagram of three electrode materials. DETAILED DESCRIPTION

[0044] In one embodiment of the present invention, the preparation method of the composite electrode material for degrading chlorinated hydrocarbon pollutants comprises the following steps:

[0045] (1) dissolving nickel nitrate hexahydrate, urea and ammonium fluoride in ultrapure water, and stirring to obtain a mixed solution;

[0046] (2) ultrasonically treating the nickel foam with hydrochloric acid, water, acetone and ethanol respectively, and drying the nickel foam;

[0047] (3) placing the nickel foam and the mixed solution in a reactor, and subjecting the mixture to a hydrothermal reaction to obtain a Ni(OH)2 / NF electrode;

[0048] (4) dissolving a palladium source and sodium chloride in ultrapure water, stirring them evenly and then performing ultrasonic treatment to uniformly disperse the palladium source;

[0049] (5) A Pt sheet was used as an anode and a Ni(OH)2 / NF electrode was used as a cathode, which were immersed in the above-mentioned palladium source mixed solution and subjected to constant current electrodeposition to obtain a Pd / Ni(OH)2 / NF electrode as an example;

[0050] (6) Similarly, a Pt sheet was used as an anode and a nickel foam was used as a cathode, which were immersed in the above-mentioned palladium source mixed solution and subjected to constant current electrodeposition to obtain a Pd / NF electrode as a comparative example.

[0051] In another embodiment of the present invention, the Pd / Ni(OH)2 / NF electrode obtained by the aforementioned preparation method is used as a hydrogenation catalyst for degrading chlorinated hydrocarbon pollutants, which is described in detail below through some specific examples and comparative examples.

[0052] Example 1

[0053] Catalyst preparation:

[0054] Weigh 0.291g nickel nitrate hexahydrate, 0.240g urea and 0.074g ammonium fluoride and dissolve them in 40mL ultrapure water, stir until clear, and add to an 80mL reactor. Ultrasonicate a 2cm×2cm nickel foam with 2mol / L hydrochloric acid, water, acetone and ethanol for 20-30min respectively to remove impurities such as surface oxide layer and grease. Dry at 60℃ for 6h after the ultrasonic treatment. Then put the nickel foam into the reactor and react at 160℃ for 4h to obtain a Ni(OH)2 / NF electrode and dry it for use. The Pt sheet is used as the anode and the Ni(OH)2 / NF electrode is used as the cathode. It is immersed in 80ml of a mixed solution of 1mM PdCl2 and 3mM NaCl, and electrodeposited at 7mA constant current and 313K for 1h to obtain a Pd / Ni(OH)2 / NF electrode. For the growth process of preparing the electrode material, see Figure 1 After electrodeposition of Pd, the crystallinity of Ni(OH)2 in the Pd / Ni(OH)2 / NF electrode was not destroyed, and the lattice degree of the material was high, see Figure 2 .

[0055] Catalyst hydrodechlorination evaluation:

[0056] The electrocatalytic hydrodechlorination reaction of TCE was carried out in a 100mL electrochemical reaction cell. The Ag / AgCl electrode was used as the reference electrode, and the Pt sheet (2cm×2cm) was used as the anode, which was placed vertically and parallel to the Pd / Ni(OH)2 / NF electrode (2cm×2cm) with a spacing of 2cm. The dechlorination experiment was carried out with TCE with an initial concentration of 20mg / L. The electrolyte was 50mM sodium sulfate solution, the reaction solution volume was 80mL, the pH was controlled to 7, and the electrolysis voltage was -1.3V. An electrochemical workstation (Shanghai Chenhua, CHI760E) was used to control the constant potential electrolysis process and perform electrochemical analysis.

[0057] The concentrations of TCE and liquid dechlorination products were determined by gas chromatography / mass spectrometry (GC / MS) using an Agilent 5977B GC / MS instrument equipped with an OI Analytical 4100 purge-trap instrument and a DB-5MS capillary (30 m×0.25 mm, 1.4 μm thick). The internal standard was fluorobenzene (MFB). The chromatographic conditions were set as follows: inlet temperature 220°C, split injection (split ratio 30:1), program temperature: 35°C (2 min) → 5°C / min → 120°C → 10°C / min → 220°C (2 min); the carrier gas was helium with a flow rate of 1.0 mL / min. At different reaction times, 0.3 mL of sample was collected with a sealed syringe for GC / MS testing. The concentration of gas phase dechlorination products was determined using a Shmadzu GC-2014C gas chromatograph equipped with a Rt-Q-BOND column (30m×10μm, 0.32mm thick). The chromatographic conditions were set as follows: inlet temperature 200℃, carrier gas nitrogen, purge flow 1.0mL / min, split injection (split ratio 10:1), column temperature 80℃, FID detector temperature 300℃, air flow 400mL / min, H2 flow 40mL / min, and make-up gas flow 30mL / min. Standard ethylene or ethane gas was injected into the electrochemical cell to draw a gas quantitative standard curve. At different reaction times, 1mL of headspace gas in the reaction cell was collected and injected into the gas chromatograph for component analysis.

[0058] The activity results of catalyst 1 are shown in Figure 3 . After 1 hour of reaction, the degradation rate of trichloroethylene was 92%, and the conversion rate of ethane was 62%; after 3 hours of reaction, the degradation rate of trichloroethylene was 99%. The main components of the liquid phase during the degradation process are trichloroethylene, as well as trace amounts of 1,1-dichloroethylene, cis-1,2-DCE and trans-1,2-DCE intermediates; the gas phase products are mainly ethane, as well as trace amounts of other alkane and olefin products. After 1 hour of reaction, the GC spectrum shows that the peak of n-butene disappears and the peak of n-butane appears, indicating that the alkane products are more stable during the degradation of TCE. It can be inferred that the basic mechanism of the reaction is that TCE undergoes rapid electrochemical reduction under the action of H*, and trace intermediates are produced in the process. Due to hydrogenation, the final product is mainly alkanes (ethane). Therefore, the degradation of trichloroethylene by the electrode prepared in Example 1 of the present invention does not cause further pollution to the environment.

[0059] Example 2

[0060] Catalyst 2 was prepared with reference to Example 1, the electrodeposition time was controlled to be 30 min, and the other parameters were the same as those in Example 1.

[0061] The activity results of catalyst 2 are as follows: after 1 hour of reaction, the degradation rate of trichloroethylene is 84%; after 3 hours of reaction, the degradation rate of trichloroethylene is 92%.

[0062] Example 3

[0063] Catalyst 3 was prepared with reference to Example 1, the electrodeposition time was controlled to be 45 min, and the other parameters were the same as those in Example 1.

[0064] The activity results of catalyst 3 are as follows: after 1 hour of reaction, the degradation rate of trichloroethylene is 90%; after 3 hours of reaction, the degradation rate of trichloroethylene is 65%.

[0065] Embodiment 4 to Embodiment 16

[0066] Examples 4 to 16 were carried out according to the experimental parameters in Table 1, and the electrode preparation method was the same as that in Example 1.

[0067] The experimental results of Examples 4 to 6 are shown in Figure 4 , the experimental results of Examples 7 to 16 are shown in Figure 5 , Figure 5 a is different external voltage, Figure 5 b is different pH, Figure 5 c is the coexisting ions added into different groundwaters, Figure 5 d is the test result of the cycling performance of Pd / Ni(OH)2 / NF under the optimal electrochemical conditions (initial pH = 7.0, electrolyte 50mM Na2SO4, initial concentration of trichloroethylene 20mg / L, applied potential = -1.3Vvs.Ag / AgCl). The electrode material Pd / Ni(OH)2 / NF of the present invention can maintain strong electrocatalytic activity in a wide pH range (pH = 3-9) and is not easily affected by Ca in actual groundwater. 2+ 、HCO3 - 、SO3 2- and Cl - It is not affected by common anions and cations, and still shows high reactivity after 6 cycles.

[0068] Table 1

[0069]

[0070] Embodiment 17

[0071] 20 mg / L trichloroethylene was introduced into real groundwater to evaluate the actual degradation effect of the catalyst Pd / Ni(OH)2 / NF on trichloroethylene-contaminated groundwater. The catalyst hydrodechlorination reaction conditions were the same as those in Example 1.

[0072] The experimental results can be found in Figure 6After 1 hour of reaction, the degradation rate of trichloroethylene was 48%; after 3 hours of reaction, the degradation rate of trichloroethylene was 88%. In real groundwater, the removal effect of trichloroethylene by the catalyst Pd / Ni(OH)2 / NF of the present invention was slightly lower than that in experimental simulated groundwater (50mM Na2SO4), but still showed good dechlorination performance.

[0073] Comparative Example 1

[0074] The nickel foam of 2cm×2cm size was ultrasonically treated with 2mol / L hydrochloric acid, water, acetone and ethanol for 20-30min to remove the surface oxide layer and impurities such as grease, and then dried at 60℃ for 6h. The Pt sheet was used as the anode and the nickel foam was used as the cathode. They were immersed in a mixed solution of 1mM PdCl2 and 3mM NaCl, and electroplated at 7mA constant current and 313K for 1h to obtain the Pd / NF electrode.

[0075] The catalyst hydrodechlorination reaction conditions are the same as those in Example 1. Figure 4 After 1 hour of reaction, the degradation rate of trichloroethylene was 52%; after 3 hours of reaction, the degradation rate of trichloroethylene was 90%.

[0076] Comparative Example 2

[0077] Weigh 0.291g nickel nitrate hexahydrate, 0.240g urea and 0.074g ammonium fluoride and dissolve them in 40mL ultrapure water, stir until clear, and add them to an 80mL reactor. Ultrasonicate the 2cm×2cm nickel foam with 2mol / L hydrochloric acid, water, acetone and ethanol for 20 to 30 minutes to remove the surface oxide layer and impurities such as grease. After the ultrasound, dry it at 60℃ for 6h. Then put the nickel foam into the reactor and react at 160℃ for 4h to obtain the Ni(OH)2 / NF electrode and dry it for use.

[0078] The catalyst hydrodechlorination reaction conditions are the same as those in Example 1. Figure 4 After 1 hour of reaction, the degradation rate of trichloroethylene was 35%; after 3 hours of reaction, the degradation rate of trichloroethylene was 65%.

[0079] It can be seen from Comparative Examples 1 to 2 and Examples 1 to 3 that the electrocatalytic performance of the Pd / Ni(OH)2 / NF electrode always remains optimal.

[0080] Compare the SEM and TEM images of the electrode materials prepared in Example 1 and Comparative Example 1, see Figure 7-8 The metal Pd on the surface of the electrode material Pd / Ni(OH)2 / NF prepared in Example 1 is more evenly dispersed, and the size effect brought about by the smaller Pd particle size means an increase in the active sites on the catalyst surface.

[0081] The XPS spectra of the electrode materials prepared in Example 1 and Comparative Example 1 are shown in FIG. Fig. 9 The Pd peak of the electrode material Pd / Ni(OH)2 / NF prepared in Example 1 has a negative shift of 0.5 eV, indicating that a relatively strong interface interaction has been formed between the Ni(OH)2 intermediate layer and Pd. The electron transfer mechanism brought about by the introduction of the Ni(OH)2 nanoarray intermediate layer can promote the enrichment of electrons on the Pd surface, which is beneficial to the active hydrogen H * The generation of ions can improve the reaction performance of the electrode.

[0082] CV graphs of the electrode material Pd / Ni(OH)2 / NF prepared in Example 1 with and without trichloroethylene added to the electrolyte ( Fig.10 a) Confirm that H * ads It is the active hydrogen species that dominates the electrode material during the electrolysis of trichloroethylene.

[0083] Comparative Example 1 and Comparative Examples 1-2 electrode materials prepared by CV graph ( Fig.10 b) The active hydrogen species H generated by the electrode material Pd / Ni(OH)2 / NF prepared in Example 1 * ads The oxidation peak area is larger, indicating the generation of H * ads The larger number confirms the superiority of the dechlorination performance of the electrode material.

[0084] Based on the above embodiments, it can be known that, as another embodiment of the present invention, the Pd / Ni(OH)2 / NF electrode can be used in the hydrodechlorination of chlorinated hydrocarbon pollutants in groundwater, more specifically, the hydrogenation reduction dechlorination of trichloroethylene in groundwater. * ads It has the ability of rapid electrochemical reduction and dechlorination under mediation, with less reaction by-products, good reaction activity and stability. After 6 cycles of use, the trichloroethylene removal rate is still maintained above 90%, and can reach up to 95%. The electrode material can maintain strong electrocatalytic activity in a wide pH range (pH = 3-9) and is not easily affected by common anions and cations in actual groundwater, showing its feasibility for the actual degradation of trichloroethylene.

[0085] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.

Claims

1. A method for preparing a composite electrode material for degrading chlorinated hydrocarbon pollutants, characterized in that: The following steps are involved: Mixing nickel nitrate hexahydrate, urea and ammonium fluoride to obtain a mixed solution, subjecting the mixed solution to a hydrothermal synthesis reaction with nickel foam, and coating a Ni(OH)2 nanoarray on the nickel foam substrate to obtain a Ni(OH)2 / NF electrode material; The Ni(OH)2 / NF electrode material is further electroplated with metal palladium to prepare a Pd / Ni(OH)2 / NF nickel-based composite electrode material with a three-dimensional rosette morphology.

2. The preparation method according to claim 1, characterized in that: The molar ratio of the nickel nitrate hexahydrate, urea and ammonium fluoride is 1:4:

2.

3. The preparation method according to claim 1, characterized in that: The hydrothermal synthesis reaction specifically includes: placing the mixed solution and nickel foam in a polytetrafluoroethylene reactor, sealing it and heating it for reaction, and then washing and drying it to obtain a Ni(OH)2 / NF electrode material based on nickel foam.

4. The preparation method according to claim 3, characterized in that: The nickel foam is pretreated before the hydrothermal synthesis reaction. Specifically, the nickel foam is ultrasonically treated with hydrochloric acid, water, acetone and ethanol respectively for 15-30 minutes to remove the surface oxide layer and impurities such as grease, and then placed in an oven for drying and then standing for use.

5. The preparation method according to claim 3, characterized in that: The hydrothermal synthesis reaction temperature is 160°C to 200°C, the heating rate is 5°C / min, and the reaction time is 4h to 6h.

6. The preparation method according to claim 1, characterized in that: The specific steps of electroplating metal palladium include: A palladium source and NaCl are mixed in water to prepare an electrolyte, and a three-electrode system is placed in the prepared electrolyte, wherein the Ni(OH)2 / NF electrode material is the working electrode, Pt is the counter electrode, and Ag / AgCl is the reference electrode. Electrodeposition is carried out at a constant current of 7 mA and 313 K for 0.5 to 1 h, and the voltage is controlled at about -0.8 V to prepare the Pd / Ni(OH)2 / NF nickel-based composite electrode material.

7. The preparation method according to claim 6, characterized in that: The palladium source is at least one of palladium chloride and palladium nitrate.

8. A composite electrode material for degrading chlorinated hydrocarbon pollutants, characterized in that: The composite electrode material is prepared by the preparation method described in any one of claims 1 to 7; Preferably, in the composite electrode material, the loading amount of the active component palladium is 2.0 wt% to 3.0 wt% based on the mass of the metal palladium.

9. Use of the composite electrode material according to claim 8 or the composite electrode material prepared by the preparation method according to any one of 1 to 7 as a catalyst in the hydrodechlorination degradation of chlorinated hydrocarbon pollutants.

10. The use according to claim 9, wherein the chlorinated hydrocarbon pollutant comprises trichloroethylene.

Citation Information

Patent Citations

  • Electrocatalytic ammonia oxidation hydrogen production electrode material as well as preparation method and application thereof

    CN111068685A

  • Metal palladium particle loaded electrode with bimetal organic framework as middle layer and preparation and application of metal palladium particle loaded electrode

    CN114956267A

  • Method for preparing Pd / Ni3S2 / NF nanosheet array electrode through in-situ vulcanization electrodeposition and EHDC method

    CN115784388A

Cited By

  • Cathode material for electrocatalytic degradation of tetracycline as well as preparation method and application of cathode material

    CN120172494A