Oxygen evolution catalyst as well as preparation method and application thereof

By constructing the NiFe base layered hydroxide core-shell structure on nickel-based materials and doping sulfur ions and tungsten ions, the problem of poor activity of precious metal catalysts under high current density is solved, and high-activity and low-cost oxygen evolution are achieved The catalyst significantly improves the efficiency of hydrogen production by electrolyzing water.

CN118932403APending Publication Date: 2024-11-12THE HONG KONG UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411129539.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing precious metal catalysts IrO2 and RuO2 have small starting potentials but high overpotentials under high current density, and their catalytic activity is not ideal, making it difficult to effectively promote the oxygen evolution reaction in electrolyzed water.

Method used

The nickel-based material is used to combine with the NiFe base layered hydroxide core-shell structure, and the electronic structure and composition are adjusted by doping sulfur ions and tungsten ions, reducing the initial overpotential, and improving conductivity and catalytic activity.

Benefits of technology

The activity and stability of the oxygen evolution catalyst are significantly improved, the initial overpotential is reduced, the oxygen evolution reaction is accelerated, and the cost is low.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932403A_ABST
    Figure CN118932403A_ABST
Patent Text Reader

Abstract

The invention provides an oxygen evolution catalyst and a preparation method and application thereof.The oxygen evolution catalyst comprises a nickel substrate material and a core-shell structure attached to the nickel substrate material, the core-shell structure comprises an inner core and an outer shell layer, the inner core comprises NiS2, the outer shell layer comprises NiFe-based layered hydroxide, and the outer shell layer comprises NiFe-based layered hydroxide. The NiFe-based layered hydroxide comprises a NiFe layered hydroxide, and sulfur ions and tungsten ions doped in the NiFe layered hydroxide. The core-shell structure is beneficial to rapid transfer of electrons, permeation of electrolyte and release of reaction gas; the sulfur ions and tungsten ions are co-doped, so that the electronic structure of metal in the NiFe layered hydroxide is improved, the binding energy of a reaction intermediate is optimized, the conductivity of the NiFe layered hydroxide is improved, and finally, the activity and stability of the oxygen evolution catalyst are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of catalyst technology, and in particular to an oxygen evolution catalyst and a preparation method and application thereof. Background Art

[0002] With the depletion of traditional fossil fuels and the increasing demand for energy, it is urgent to find suitable clean energy. Hydrogen is considered to be the most promising candidate due to its high energy density and environmental friendliness. At present, water electrolysis is an attractive large-scale hydrogen production strategy, which includes hydrogen evolution reaction and oxygen evolution reaction. However, due to the slow multi-electron process and high activation barrier, the oxygen evolution reaction inhibits the commercial application of water electrolysis. Therefore, researchers are committed to finding suitable oxygen evolution catalysts to solve the problem of water electrolysis.

[0003] At present, the commonly used oxygen evolution catalysts are precious metal products IrO2 and RuO2. Precious metal products IrO2 and RuO2 as oxygen evolution catalysts have good performance at high current density (100 mA cm -2 , 500 mA cm -2 , 1000 mA cm -2 ), its initial potential is small, but the overpotential is high, and the catalytic activity is not ideal. Therefore, researchers are committed to developing high-activity, low-cost oxygen evolution catalysts. Summary of the invention

[0004] Based on this, it is necessary to provide an oxygen evolution catalyst and a preparation method and application thereof, which can have high catalytic activity at high current density.

[0005] In one aspect of the present application, an oxygen evolution catalyst is provided, which includes a nickel base material and a core-shell structure attached to the nickel base material, the core-shell structure includes an inner core and an outer shell layer, the inner core includes NiS2, the outer shell layer includes a NiFe-based layered hydroxide, and the NiFe-based layered hydroxide includes NiFe layered hydroxide and sulfur ions and tungsten ions doped in the NiFe layered hydroxide.

[0006] In the above oxygen evolution catalyst, countless core-shell structures are attached to the nickel base material, and this core-shell structure facilitates the rapid transfer of electrons, the penetration of electrolytes, and the release of reaction gases, thereby improving the electrocatalytic activity of the oxygen evolution catalyst. NiS2 on the surface of the nickel base material serves as the core of the core-shell structure, which can improve the electrical conductivity of the base material. The NiFe-based layered hydroxide includes NiFe layered hydroxides and sulfide ions and tungsten ions doped in the NiFe layered hydroxides. The doping of sulfide ions and tungsten ions can adjust the composition of the NiFe layered hydroxides; the tungsten ions doped in the NiFe layered hydroxides can modify the electronic structure and produce more active sites, thereby reducing the initial overpotential and accelerating the oxygen evolution reaction. Tungsten ion doping can also enhance the conductivity of the NiFe layered hydroxides. Sulfide ions doped in the NiFe layered hydroxides help adjust the electronic structure and produce metal vacancies, thereby further improving the conductivity of the NiFe layered hydroxides and optimizing the electrochemical oxygen evolution activity of the NiFe layered hydroxides. The sulfur ions and tungsten ions in the NiFe layered hydroxide are co-doped with anions and cations, which improves the electronic structure of the metal in the NiFe layered hydroxide, optimizes the binding energy of the reaction intermediates, improves the electrical conductivity of the NiFe layered hydroxide, and ultimately significantly improves the activity and stability of the oxygen evolution catalyst. The oxygen evolution catalyst of the above structure has achieved unexpected results in improving the activity and stability of the oxygen evolution catalyst. The oxygen evolution catalyst of the present application also has the advantage of low cost.

[0007] In some embodiments, the thickness of the outer layer is 1-2 µm.

[0008] In some embodiments, the content of sulfide ions is 16 wt%~20wt%.

[0009] In some embodiments, the content of the tungsten ions is 6 wt% to 10 wt%.

[0010] In some embodiments, the nickel base material is nickel foam, which has a fluffy porous structure.

[0011] The second aspect of the present application provides a method for preparing an oxygen evolution catalyst, comprising the following steps:

[0012] S1, dissolving an iron source, a nickel source, ammonium fluoride, urea and a tungsten source in a solvent and mixing them to obtain a metal salt precursor solution;

[0013] S2, adding the nickel base material to the metal salt precursor solution for hydrothermal treatment to obtain a hydrothermal treatment product;

[0014] S3, subjecting the hydrothermal treatment product to a sulfidation treatment to obtain the oxygen evolution catalyst.

[0015] The aforementioned preparation method introduces tungsten ions by wet chemical method, introduces sulfur ions by sulfidation treatment, and then co-dopes sulfur ions and tungsten ions into NiFe layered hydroxide. This method of co-doping with anions and cations improves the activity and stability of the oxygen evolution catalyst. In the aforementioned preparation method, each metal salt precursor is first uniformly dissolved in a solvent by wet chemical method, and then a layered hydroxide in which the metal is uniformly dispersed is obtained by hydrothermal treatment, and then the hydrothermal treatment product is sulfided to obtain an oxygen evolution catalyst co-doped with sulfur ions and tungsten ions. The aforementioned preparation method significantly improves the conductivity of the oxygen evolution catalyst by co-doping with sulfur ions and tungsten ions, improves the electronic structure of the oxygen evolution catalyst metal, optimizes the binding energy of the reaction intermediates, and ultimately promotes the reaction kinetics of oxygen evolution and improves the stability of the catalyst, so that the prepared oxygen evolution catalyst has a very high oxygen evolution catalytic performance. Moreover, the preparation method of the present application has a simple and efficient process flow.

[0016] The above-mentioned preparation method uses a combination of hydrothermal method and high-temperature sulfurization to synthesize the oxygen evolution catalyst. The specific synthesis process is divided into two steps. The first step is to synthesize NiFeW by hydrothermal treatment, and the second step is to obtain the oxygen evolution catalyst by sulfurization treatment. Among them, during the sulfurization treatment, on the one hand, the outer NiFeW is sulfurized, and on the other hand, the surface of the internal nickel base material is sulfurized to obtain NiS2, thereby improving the conductivity of the base material and ultimately improving the activity of the oxygen evolution catalyst.

[0017] In some embodiments, in S3, the temperature of the sulfurization treatment is 180°C to 380°C.

[0018] In some embodiments, in S1, the iron source, the nickel source and the tungsten source are mixed in a molar ratio of iron element, nickel element and tungsten element of 1:2-6:0.5-5.

[0019] In some embodiments, S1 satisfies at least one of the following conditions:

[0020] (1) The iron source includes ferric nitrate nonahydrate;

[0021] (2) The nickel source includes nickel nitrate hexahydrate;

[0022] (3) The tungsten source includes tungsten hexachloride;

[0023] (4) The solvent is an alcohol solvent.

[0024] In some implementation modes, in S2, at least one of the following conditions is satisfied:

[0025] (1) The hydrothermal treatment temperature is 120°C to 180°C;

[0026] (2) The hydrothermal treatment time is 5h~20h.

[0027] In some embodiments, at least one of the following conditions is satisfied in S3:

[0028] (1) The temperature of the vulcanization treatment is 200°C to 350°C;

[0029] (2) The holding time of the vulcanization treatment is 1h~5h.

[0030] In some embodiments, in S3, sulfur powder is further added to the sulfurization treatment, and the mass ratio of the hydrothermal treatment product to the sulfur powder is 1:1-5.

[0031] In some embodiments, in S2, the nickel base material is nickel foam.

[0032] The third aspect of the present application provides an application of the oxygen evolution catalyst as described in the first aspect, wherein the oxygen evolution catalyst is applied to water electrolysis to produce hydrogen or a fuel cell.

[0033] The fourth aspect of the present application provides a hydrogen production device by electrolysis of water, comprising the oxygen evolution catalyst as described in the first aspect and the oxygen evolution catalyst prepared by the preparation method as described in the second aspect.

[0034] A fifth aspect of the present application provides a fuel cell, comprising the oxygen evolution catalyst as described in the first aspect and the oxygen evolution catalyst prepared by the preparation method as described in the second aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Polarization curves of the oxygen evolution catalyst prepared in Example 1 and the samples in Comparative Examples 1 to 3 in 1 M KOH.

[0036] Figure 2 The figure is a comparison diagram of the overpotential of the oxygen evolution catalyst prepared in Example 1 and the samples in Comparative Examples 1 to 3.

[0037] Figure 3 This is a stability curve of the oxygen evolution catalyst prepared in Example 1 in 1 M KOH.

[0038] Figure 4 This is a scanning electron microscope image of the oxygen evolution catalyst prepared in Example 1. DETAILED DESCRIPTION

[0039] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0041] Layered double hydroxides are considered to be a promising oxygen evolution catalyst to replace precious metal catalysts in alkaline solutions due to their highly tunable structure, enhanced host-guest interactions, and atomically dispersed active sites. So far, the oxygen evolution performance of NiFe-based layered double hydroxides is better than that of NiCo-based layered double hydroxides and CoFe-based layered double hydroxides. However, the low conductivity and low density of active sites limit the electrocatalytic activity of NiFe-based layered double hydroxide materials. Currently, there is an urgent need for an oxygen evolution catalyst with excellent activity and stability at high current density and a simple and efficient synthesis method.

[0042] In a first aspect of the present application, an oxygen evolution catalyst is provided, and the oxygen evolution catalyst will be described in detail below in conjunction with a preparation method.

[0043] In one embodiment of the present application, an oxygen evolution catalyst is provided, which includes a nickel base material and a core-shell structure attached to the nickel base material, the core-shell structure includes an inner core and an outer shell layer, the inner core includes NiS2, the outer shell layer includes a NiFe-based layered hydroxide, and the NiFe-based layered hydroxide includes NiFe layered hydroxide and sulfur ions and tungsten ions doped in the NiFe layered hydroxide.

[0044] In the above oxygen evolution catalyst, countless core-shell structures are attached to the nickel base material, and this core-shell structure facilitates the rapid transfer of electrons, the penetration of electrolytes, and the release of reaction gases, thereby improving the electrocatalytic activity of the oxygen evolution catalyst. NiS2 on the surface of the nickel base material serves as the core of the core-shell structure, which can improve the electrical conductivity of the base material. The NiFe-based layered hydroxide includes NiFe layered hydroxides and sulfide ions and tungsten ions doped in the NiFe layered hydroxides. The doping of sulfide ions and tungsten ions can adjust the composition of the NiFe layered hydroxides; the tungsten ions doped in the NiFe layered hydroxides can modify the electronic structure and produce more active sites, thereby reducing the initial overpotential and accelerating the oxygen evolution reaction. Tungsten ion doping can also enhance the conductivity of the NiFe layered hydroxides. Sulfide ions doped in the NiFe layered hydroxides help adjust the electronic structure and produce metal vacancies, thereby further improving the conductivity of the NiFe layered hydroxides and optimizing the electrochemical oxygen evolution activity of the NiFe layered hydroxides. The sulfur ions and tungsten ions in the NiFe layered hydroxide are co-doped with anions and cations, which improves the electronic structure of the metal in the NiFe layered hydroxide, optimizes the binding energy of the reaction intermediates, improves the electrical conductivity of the NiFe layered hydroxide, and ultimately significantly improves the activity and stability of the oxygen evolution catalyst. The oxygen evolution catalyst of the above structure has achieved unexpected results in improving the activity and stability of the oxygen evolution catalyst. The oxygen evolution catalyst of the present application also has the advantage of low cost.

[0045] In some embodiments, the outer layer has a thickness of 1 to 2 µm.

[0046] In some embodiments, the content of sulfide ions is 16wt%~20wt%.

[0047] Understandably, sulfur ions account for 16wt% to 20wt% of the weight of the oxygen evolution catalyst.

[0048] Furthermore, the content of the sulfide ion is preferably 18wt%~20wt%.

[0049] In some embodiments, the content of the tungsten ions is 6wt%~10wt%.

[0050] Specifically, tungsten ions account for 6 wt% to 10 wt% of the weight of the oxygen evolution catalyst.

[0051] Furthermore, the content of the tungsten ions is preferably 8.4 wt% to 10 wt%.

[0052] In some embodiments, the nickel base material of the oxygen evolution catalyst is nickel foam.

[0053] The second aspect of the present application provides a method for preparing an oxygen evolution catalyst, comprising the following steps:

[0054] S1, dissolving an iron source, a nickel source, ammonium fluoride, urea and a tungsten source in a solvent and mixing them to obtain a metal salt precursor solution;

[0055] S2, adding the nickel base material to the metal salt precursor solution for hydrothermal treatment to obtain a hydrothermal treatment product;

[0056] S3, subjecting the hydrothermal treatment product to a sulfidation treatment to obtain the oxygen evolution catalyst.

[0057] The aforementioned preparation method introduces tungsten ions by wet chemical method, introduces sulfur ions by sulfidation treatment, and then co-dopes sulfur ions and tungsten ions into NiFe layered hydroxide. This method of co-doping with anions and cations improves the activity and stability of the oxygen evolution catalyst. In the aforementioned preparation method, each metal salt precursor is first uniformly dissolved in a solvent by wet chemical method, and then a layered hydroxide in which the metal is uniformly dispersed is obtained by hydrothermal treatment, and then the hydrothermal treatment product is sulfided to obtain an oxygen evolution catalyst co-doped with sulfur ions and tungsten ions. The aforementioned preparation method significantly improves the conductivity of the oxygen evolution catalyst by co-doping with sulfur ions and tungsten ions, improves the electronic structure of the oxygen evolution catalyst metal, optimizes the binding energy of the reaction intermediates, and ultimately promotes the reaction kinetics of oxygen evolution and improves the stability of the catalyst, so that the prepared oxygen evolution catalyst has a very high oxygen evolution catalytic performance. Moreover, the preparation method of the present application has a simple and efficient process flow.

[0058] The above-mentioned preparation method uses a combination of hydrothermal method and high-temperature sulfurization to synthesize the oxygen evolution catalyst. The specific synthesis process is divided into two steps. The first step is to synthesize NiFeW by hydrothermal treatment, and the second step is to obtain the oxygen evolution catalyst by sulfurization treatment. Among them, during the sulfurization treatment, on the one hand, the outer NiFeW is sulfurized, and on the other hand, the surface of the internal nickel base material is sulfurized to obtain NiS2, thereby improving the conductivity of the nickel base material and ultimately improving the activity of the oxygen evolution catalyst.

[0059] In some embodiments, in S3, the precursor metal salt in the hydrothermal treatment product is removed before the sulfidation treatment.

[0060] In some embodiments, in S1, the iron source, the nickel source and the tungsten source are mixed in a molar ratio of iron element, nickel element and tungsten element of 1:2~6:0.5~5. By optimizing the mixing ratio of the tungsten source, the nickel source and the iron source, a more active NiFeW layer can be obtained; under this ratio, the NiFe electronic structure is fully adjusted without changing the morphology and lattice of the product, which is beneficial to the discharge of the product gas and further improves the activity of the oxygen evolution catalyst.

[0061] In some embodiments, in S1, the molar ratio of the iron source, the nickel source, the ammonium fluoride, the urea and the tungsten source is 1: 2~6: 1~4: 5~15: 0.5~5. Under this ratio, the electronic structure of NiFe is fully adjusted without changing the morphology and lattice of the product, which is beneficial to the discharge of the product gas and further improves the activity of the oxygen evolution catalyst.

[0062] The molar ratio of the iron source, the nickel source, the ammonium fluoride, the urea and the tungsten source is preferably 1:3-6:1-4:5-15:2-5.

[0063] In some embodiments, in S1, the iron source is ferric nitrate nonahydrate.

[0064] In some embodiments, in S1, the nickel source is nickel nitrate hexahydrate.

[0065] In some embodiments, in S1, the tungsten source is tungsten hexachloride.

[0066] In some embodiments, in S1, the solvent is an alcohol solvent.

[0067] In some embodiments, in S1, the solvent is ethanol and / or methanol.

[0068] In some embodiments, in S1, the metal salt precursor in the solvent is mixed uniformly by stirring and ultrasonication, the stirring time is 0.5h~2h, and the ultrasonication time is 0.5h~2h. The metal salt precursor in the solvent is mixed uniformly by stirring and ultrasonication, which is conducive to obtaining a layered hydroxide with uniformly dispersed metal ions.

[0069] In some embodiments, in S2, the hydrothermal treatment temperature is 120°C to 180°C.

[0070] As an example, the hydrothermal treatment temperature can be 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C and 180°C, or a range consisting of any two of the aforementioned values ​​as end values.

[0071] In some embodiments, in S2, the hydrothermal treatment time is 5 h to 20 h.

[0072] As an example, the hydrothermal treatment time can be 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h and 20h, or within a range consisting of any two of the aforementioned values ​​as end values.

[0073] In some embodiments, in S2, the hydrothermal treatment is carried out in a 50 ml reactor.

[0074] In some embodiments, in S2, before the base material is added to the mixed solution, the base material is first placed in a 1-4 M dilute hydrochloric acid solution for ultrasonic cleaning for 10 min to 30 min, then cleaned in ethanol for 10 min to 30 min, and then ultrasonically cleaned in water for 10 min to 30 min. The base material needs to be cleaned before adding to the mixed solution.

[0075] In some embodiments, in S2, the nickel base material is nickel foam.

[0076] It is understood that during the sulfurization treatment, on the one hand, the outer NiFeW is sulfurized to form a NiFeWS layer, and on the other hand, the internal nickel foam surface is also sulfurized to obtain NiS2. The NiFeWS layer wraps the NiS2, and the inside of the nickel foam is not sulfurized. The sulfurized part of the nickel foam is closely connected with the unsulfurized part to form a whole, thereby improving the conductivity of the nickel foam and ultimately improving the activity of the oxygen evolution catalyst.

[0077] In some embodiments, in S3, the sulfurization treatment temperature is 180°C to 380°C.

[0078] As an example, the sulfurization treatment temperature can be 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, 240°C, 245°C, 250°C, 255°C, 260°C, 265°C, 270°C, 275°C, 280°C, 285°C, 290°C, 295°C, 300°C, 305°C, 310°C, 315°C, 320°C, 325°C, 330°C, 335°C and 340°C, 345°C, 350°C, 355°C, 360°C, 365°C, 370°C, 375°C and 380°C, or in a range consisting of any two of the foregoing values ​​as end values.

[0079] Furthermore, the sulfurization temperature is preferably 200° C. to 350° C. The sulfurization process in the temperature range of 200° C. to 350° C. can improve the conductivity of the oxygen evolution catalyst on the one hand, and can also adjust the electronic structure of the oxygen evolution catalyst and optimize the binding energy of the intermediate on the other hand, so that the prepared oxygen evolution catalyst exhibits higher oxygen evolution catalytic activity, stability and physical and chemical properties.

[0080] In some embodiments, in S3, the vulcanization treatment holding time is 1 h to 5 h.

[0081] As an example, the vulcanization treatment holding time can be 1h, 1.5h, 2.0h, 2.5h, 3.0h, 3.5h, 4.0h, 4.5h, 5.0h, or a range consisting of any two of the aforementioned values ​​as end values.

[0082] Furthermore, the holding time of the sulfurization treatment is preferably 1 h to 3 h. Within this holding time, the sulfurization effect is better, and the catalytic activity and stability of the obtained oxygen evolution catalyst are better.

[0083] In some embodiments, in S3, in the sulfurization treatment, the mass ratio of the hydrothermal treatment product to sulfur powder is 1:1-5.

[0084] As an example, the mass ratio of the hydrothermal treatment product to sulfur powder can be 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4.0, 1:4.5 and 1:5, or within a range consisting of any two of the aforementioned values ​​as end values.

[0085] Furthermore, the mass ratio of the hydrothermal treatment product to sulfur powder is preferably 1:3-5.

[0086] In some embodiments, in S3, an alcohol solvent is used to remove unreacted precursor metal salt in the hydrothermal treatment product before the sulfidation treatment.

[0087] Furthermore, the nickel foam after the hydrothermal treatment is taken out, and the unreacted metal salt precursor metal salt is washed with ethanol or methanol.

[0088] In some embodiments, in S3, the sulfurization treatment is carried out in a tubular furnace, with a slow purge of sulfur vapor, and the atmosphere is an inert gas atmosphere. The present invention combines a hydrothermal method with high-temperature sulfurization. The specific synthesis process is divided into two steps, the first step is to synthesize NiFeW by hydrothermal method, and the second step is to obtain the final product by heat treatment sulfurization. By treating the reactants with high-temperature sulfurization, the slow purge of sulfur vapor sulfurizes the outer NiFeW layer on the one hand, and also sulfurizes the internal nickel foam surface on the other hand, thereby improving the conductivity of the substrate.

[0089] A third aspect of the present application provides an application of the oxygen evolution catalyst as described in the first aspect, wherein the oxygen evolution catalyst is applied to water electrolysis to produce hydrogen or a fuel cell.

[0090] A fourth aspect of the present application provides a hydrogen production device by electrolysis of water, comprising the oxygen evolution catalyst as described in the first aspect and the oxygen evolution catalyst prepared by the preparation method as described in the second aspect.

[0091] A fifth aspect of the present application provides a fuel cell, comprising the oxygen evolution catalyst as described in the first aspect and the oxygen evolution catalyst prepared by the preparation method as described in the second aspect.

[0092] The following are specific embodiments.

[0093] Example 1

[0094] An oxygen evolution catalyst is prepared by the following method:

[0095] (1) Ferric nitrate nonahydrate, nickel nitrate hexahydrate, ammonium fluoride, urea and tungsten hexachloride in a molar ratio of 1:3:1:5:2 were mixed and dissolved in 30 ml of ethanol solvent; then a uniformly dispersed mixed solution was obtained by stirring and ultrasonication; the stirring time was 0.5 hour, and the ultrasonication time was 0.5 hour.

[0096] (2) The mixed solution of step (1) and the cleaned nickel foam are placed in a 50 ml reactor and reacted at 180° C. for 10 hours. The nickel foam cleaning process is as follows: the nickel foam is placed in a 3 M dilute hydrochloric acid solution for 30 minutes, then cleaned in ethanol for 30 minutes, and finally ultrasonically cleaned in water for 30 minutes.

[0097] (3) Take out the nickel foam from step (2) and wash the unreacted metal salt precursor with ethanol or methanol.

[0098] (4) The product of step (3) and sulfur powder in a mass ratio of 1:3 are placed in a tubular furnace for sulfurization treatment at 250° C. in an inert gas atmosphere for 1 hour to obtain an oxygen evolution catalyst (NiS2@NiFeWS / NF) with high catalytic activity and stability.

[0099] Example 2

[0100] The preparation method of Example 2 is substantially the same as that of Example 1, except that the sulfurization treatment temperature is 200°C.

[0101] Example 3

[0102] The preparation method of Example 3 is substantially the same as that of Example 1, except that the sulfurization treatment temperature is 350°C.

[0103] Example 4

[0104] The preparation method of Example 4 is substantially the same as that of Example 1, except that the sulfurization treatment temperature is 180°C.

[0105] The sulfurization temperature of Example 4 is relatively low, resulting in a lower sulfur doping content, so the oxygen evolution performance is relatively weak.

[0106] Example 5

[0107] The preparation method of Example 5 is substantially the same as that of Example 1, except that the sulfurization treatment temperature is 380°C.

[0108] Example 6

[0109] The preparation method of Example 6 is basically the same as the preparation method of Example 1, except that the holding time of the vulcanization treatment is 5 hours.

[0110] Example 7

[0111] The preparation method of Example 7 is substantially the same as that of Example 1, except that:

[0112] Ferric nitrate nonahydrate, nickel nitrate hexahydrate, ammonium fluoride, urea and tungsten hexachloride in a molar ratio of 1:6:4:15:5 are mixed and dissolved in a solvent.

[0113] Comparative Example 1

[0114] The NFs were subjected to electrochemical tests in 1 M KOH solution.

[0115] Comparative Example 2

[0116] The Ni3Fe / NF was subjected to electrochemical testing in 1 M KOH solution.

[0117] Comparative Example 3

[0118] The Ni3FeW / NF was subjected to electrochemical testing in 1 M KOH solution.

[0119] The oxygen evolution catalysts prepared in Examples 1 to 7 and Comparative Examples 1 to 3 were subjected to electrochemical tests using 1 M KOH solution. The test results are shown in Figure 1 , Figure 2 , Figure 3 , Figure 4 and Table 1 below.

[0120] The test conditions for each performance test item are conventional three-electrode system, the working electrode is the prepared material, the reference electrode is Hg / HgO electrode, and the counter electrode is carbon rod electrode. The electrolyte is 1M KOH. The electrochemical activity test is carried out on Chenhua 660 electrochemical workstation with a scan rate of 5 mV s -1 The electrochemical stability test was performed at a constant current (1000 mA cm -2 ) for a period of time and observe the voltage stability.

[0121] Table 1

[0122]

[0123] from Figure 1 , Figure 2As shown in Table 1, the oxygen evolution catalyst prepared in Example 1 can achieve a current density of 500 mA cm in 1 M KOH solution. -2 The overpotential of Example 1 is 302.3 mV; the overpotential of NF in Comparative Example 1 is 1006.8 mV; the overpotential of Ni3Fe / NF in Comparative Example 2 is 421.6 mV; the overpotential of Ni3FeW / NF in Comparative Example 3 is 363.4 mV. It can be seen that the overpotential of Example 1 is significantly lower than that of Comparative Examples 1 to 3, and better catalytic activity is obtained.

[0124] from Figure 3 It can be seen that the oxygen evolution catalyst prepared in Example 1 was subjected to an electrochemical test in a 1 M KOH solution. The oxygen evolution catalyst showed an ultra-long voltage stability in the 1 M KOH solution, that is, at 1000 mA cm -2 The voltage remained stable for 1000 hours at a current density of 1000 mA cm -2 The voltage remained stable for 500 hours at a current density of , which was significantly lower than that in Example 1.

[0125] The scanning electron microscope image of the oxygen evolution catalyst prepared in Example 1 is as follows: Figure 4 As shown, it exhibits a fluffy and porous nanosheet structure, which is conducive to the contact between the electrolyte and the active sites and the rapid discharge of the product gas.

[0126] It can be seen that the oxygen evolution catalyst of the present application is doped with anionic sulfur and cationic tungsten, and the co-doping of anions and cations significantly improves the conductive properties of the oxygen evolution catalyst, improves the electronic structure of the metal in the oxygen evolution catalyst, optimizes the binding energy of the reaction intermediates, and ultimately improves the activity and stability of the oxygen evolution catalyst.

[0127] As can be seen from Table 1 above, the sulfurization temperature in Example 4 is relatively low, and the sulfur content of the obtained oxygen evolution catalyst is less than that in Example 1. Therefore, the overpotential of the oxygen evolution catalyst obtained in Example 4 is higher than that in Example 1, and the catalytic activity is lower than that in Example 1; because the sulfurization temperature in Example 5 is relatively high, resulting in an increase in the sulfur doping content, although the obtained oxygen evolution catalyst has good catalytic activity, the mechanical properties are affected to a certain extent. The sulfurization time in Example 6 is relatively long, and although the obtained oxygen evolution catalyst has good catalytic activity, the mechanical properties are also affected to a certain extent. It has been verified that when the sulfurization treatment temperature is 200℃~350℃ and the holding time of the sulfurization treatment is 1h~3h, the catalytic activity and stability of the obtained oxygen evolution catalyst are significantly improved.

[0128] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0129] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. An oxygen evolution catalyst, characterized in that The oxygen evolution catalyst comprises a nickel base material and a core-shell structure attached to the nickel base material, wherein the core-shell structure comprises an inner core and an outer shell layer, wherein the inner core comprises NiS2, and the outer shell layer comprises a NiFe-based layered hydroxide, wherein the NiFe-based layered hydroxide comprises NiFe layered hydroxide and sulfur ions and tungsten ions doped in the NiFe layered hydroxide.

2. The oxygen evolution catalyst according to claim 1, characterized in that The thickness of the outer layer is 1~2μm.

3. The oxygen evolution catalyst according to claim 1, characterized in that The content of the sulfide ion is 16 wt%~20wt%.

4. The oxygen evolution catalyst according to claim 1, characterized in that The content of the tungsten ions is 6 wt% to 10 wt%.

5. The oxygen evolution catalyst according to any one of claims 1 to 4, characterized in that The nickel base material is nickel foam.

6. A method for preparing an oxygen evolution catalyst, characterized in that: The following steps are involved: S1, dissolving an iron source, a nickel source, ammonium fluoride, urea and a tungsten source in a solvent and mixing them to obtain a metal salt precursor solution; S2, adding the nickel base material to the metal salt precursor solution for hydrothermal treatment to obtain a hydrothermal treatment product; S3, subjecting the hydrothermal treatment product to a sulfidation treatment to obtain the oxygen evolution catalyst.

7. The method for preparing an oxygen evolution catalyst according to claim 6, characterized in that: In S3, the temperature of the vulcanization treatment is 180°C to 380°C.

8. The method for preparing an oxygen evolution catalyst according to claim 6, characterized in that: In S1, the iron source, the nickel source and the tungsten source are mixed in a molar ratio of iron element, nickel element and tungsten element of 1:2-6:0.5-5.

9. The method for preparing an oxygen evolution catalyst according to claim 6, characterized in that: The S1 satisfies at least one of the following conditions: (1) The iron source includes ferric nitrate nonahydrate; (2) The nickel source includes nickel nitrate hexahydrate; (3) The tungsten source includes tungsten hexachloride; (4) The solvent is an alcohol solvent.

10. The method for preparing an oxygen evolution catalyst according to claim 6, characterized in that: In S2, at least one of the following conditions is met: (1) The hydrothermal treatment temperature is 120°C to 180°C; (2) The hydrothermal treatment time is 5h~20h.

11. The method for preparing an oxygen evolution catalyst according to any one of claims 6 to 10, characterized in that: S3 satisfies at least one of the following conditions: (1) The temperature of the vulcanization treatment is 200°C to 350°C; (2) The holding time of the vulcanization treatment is 1h~5h.

12. The method for preparing an oxygen evolution catalyst according to any one of claims 6 to 10, characterized in that: In S3, sulfur powder is further added in the sulfurization treatment, and the mass ratio of the hydrothermal treatment product to the sulfur powder is 1:1-5.

13. The method for preparing an oxygen evolution catalyst according to any one of claims 6 to 10, characterized in that: In S2, the nickel base material is nickel foam.

14. Use of the oxygen evolution catalyst according to any one of claims 1 to 5, characterized in that: The oxygen evolution catalyst is applied to water electrolysis to produce hydrogen or fuel cells.

15. A hydrogen production device by electrolysis of water, characterized in that: The invention comprises the oxygen evolution catalyst as claimed in any one of claims 1 to 5 and the oxygen evolution catalyst prepared by the preparation method as claimed in any one of claims 6 to 13.

16. A fuel cell, characterized in that: The invention comprises the oxygen evolution catalyst as claimed in any one of claims 1 to 5 and the oxygen evolution catalyst prepared by the preparation method as claimed in any one of claims 6 to 13.

Citation Information

Cited By

  • Preparation method and application of nickel-based electrocatalyst rich in multi-vacancy defects

    CN119710806A