Method for preparing iron-doped CoNiFe-LDH / NF nanowire electrode and co-producing aviation fuel component by lignin-based fuel cell

Through iron-doped CoNiFe-LDH/NF nanowire electrodes, the efficient electrocatalytic oxidation and directional depolymerization are achieved in lignin-based fuel cells, and the combined production of aviation fuel components is solved, which solves the problems of low catalyst activity and waste of resources and improves fuel Battery performance and resource utilization efficiency.

CN119069723AActive Publication Date: 2024-12-03GUANGDONG UNIV OF TECH +1

Patent Information

Application Number
CN202411460718.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-12-03
Estimated Expiration
2044-10-18

AI Technical Summary

Technical Problem

The existing lignin fuel cells have problems such as low catalyst activity, slow electron transfer rate, and complex and difficult to utilize products. The existing pyrolysis method fails to effectively utilize the bond fracture energy in lignin, resulting in waste of resources.

Method used

Using iron-doped CoNiFe-LDH/NF nanowire electrodes, nanowires are grown on the surface of foam nickel by hydrothermal method, and as a high-performance electrocatalyst, lignin-based fuel cell is constructed, and lignin is depolymerized through electrocatalytic oxidation, and lignin is depolymerized in a directionally. Aviation fuel precursor is produced, and the aviation fuel components are further prepared by hydrodeoxygenation treatment.

Benefits of technology

Improve the electrocatalytic activity and electron transfer rate of lignin-based fuel cells, realize efficient lignin degradation and preparation of aviation fuel components, improve fuel cell performance and product selectivity, simplify power generation processes, and reduce energy consumption .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069723A_ABST
    Figure CN119069723A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing an iron-doped CoNiFe-LDH / NF nanowire electrode and co-producing an aviation fuel component by a lignin-based fuel cell, and belongs to the field of high-value utilization of lignin. The preparation method of the CoNiFe-LDH / NF nanowire electrode comprises the following steps: dissolving a Co source, a Ni source, a Fe source, urea and ammonium fluoride in water to obtain a hydrothermal reaction solution; and foamed nickel is placed in the hydrothermal reaction solution for a hydrothermal reaction, and the CoNiFe-LDH / NF nanowire electrode is obtained. A lignin-based fuel cell prepared from the electrode has better lignin degradation activity, and lignin macromolecules can be induced to be efficiently and directionally depolymerized into an aviation fuel precursor, so that various properties of the lignin-based fuel cell and the selectivity of a product can be improved; the co-produced aviation fuel oil precursor can be used for preparing the aviation fuel oil component through hydrodeoxygenation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of high-value utilization of lignin, and in particular to a method for preparing an iron-doped CoNiFe-LDH / NF nanowire electrode and co-producing aviation fuel components in a lignin-based fuel cell. Background Art

[0002] In recent years, the trend of reducing the use of fossil fuels has become increasingly obvious internationally, and the development and utilization of clean energy has gradually received attention. As the most abundant form of biomass on the earth, lignocellulose is considered to be one of the most promising raw materials for power generation. Fuel cells can directly convert the energy of lignocellulose into electrical energy without being limited by the efficiency of the Carnot cycle. However, although a series of lignocellulose fuel cells have been developed in the prior art, there are still various problems that hinder their large-scale application. For example, solid compound fuel cells (SOFCs), microbial fuel cells (MFCs), biomass liquid flow fuel cells (BFFCs), etc., use high temperature, redox couple mediation or microbial catalysis to degrade biomass for power generation. Solid oxide fuel cells (SOFCs) are not suitable for large-scale promotion because of the huge energy consumption caused by high temperature. Microbial fuel cells (MFCs) constructed by microbial degradation of lignin for power generation have a low power density (<0.1mW / cm 2 ). In comparison, biomass flow fuel cells have attracted widespread attention due to their high power density, low operating temperature, and wide applicability, but there is still room for further improvement in aspects such as lignin degradation activity.

[0003] At present, electrocatalysis technology has been widely used in various research fields to accelerate charge transfer at the electrode / electrolyte interface, such as hydrogen fuel cells, carbon dioxide conversion and water electrolysis. Therefore, the use of electrocatalysts is an effective way to solve the slow reaction kinetics and charge transfer between electrodes and electrolytes. However, in the field of biomass liquid flow fuel cells using lignin as fuel, the existing electrocatalysts have low activity in catalyzing lignin degradation, slow electron transfer rate, and complex products after power generation, which are difficult to further utilize and still need further improvement. Therefore, it is urgent to develop an electrocatalyst with high activity, high selectivity and high electron transfer rate, and to directionally depolymerize lignin to form valuable products while improving fuel cell performance.

[0004] Converting biomass into aviation fuel components can effectively maintain carbon balance, improve the atmospheric environment, achieve energy conservation and emission reduction, and adjust the energy structure. Biomass aviation fuel is chemically identical to traditional fossil fuel and can be mixed with existing aviation fuel without modifying the aircraft. Aviation fuel is mainly composed of a variety of chain hydrocarbons, cycloalkanes, and aromatic compounds from C8 to C16, and its specific composition varies depending on the manufacturer and raw materials. At present, most of the depolymerization of lignin is achieved through pyrolysis. This method does not collect the energy of the broken bonds in lignin, resulting in a waste of resources. The European Union stipulates that by 2025, the proportion of sustainable aviation fuel used in flights departing from EU airports must reach at least 2%, and the goal is to reach 70% by 2050. Therefore, it is urgent to develop a method for efficiently converting biomass into aviation fuel. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing an iron-doped CoNiFe-LDH / NF nanowire electrode and co-producing aviation fuel components in a lignin-based fuel cell, so as to solve the above-mentioned problems in the background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] One of the technical solutions of the present invention is to provide a method for preparing a CoNiFe-LDH / NF nanowire electrode, comprising the following steps:

[0008] The Co source, the Ni source, the Fe source, the urea and the ammonium fluoride are dissolved in water to obtain a hydrothermal reaction solution; the foamed nickel is placed in the hydrothermal reaction solution to carry out a hydrothermal reaction to obtain the CoNiFe-LDH / NF nanowire electrode.

[0009] Preferably, the Co source is Co(NO 3 ) 2 ; The Ni source is NiCl 2 ; The Fe source is FeCl 3 ; the Co(NO 3 ) 2 、NiCl 2 、FeCl 3 , the molar ratio of urea and ammonium fluoride is (1-6):(1-6):(0.2-2):(4-20):(4-20).

[0010] More preferably, the Co(NO 3 ) 2 、NiCl 2 、FeCl 3 , urea and ammonium fluoride have a molar ratio of 4:2:1:10:10.

[0011] Preferably, the temperature of the hydrothermal reaction is 20-200° C., and the time is 1-20 h.

[0012] More preferably, the temperature of the hydrothermal reaction is 50-150° C., and the time is 5-7 hours.

[0013] The second technical solution of the present invention is to provide a CoNiFe-LDH / NF nanowire electrode obtained according to the above preparation method.

[0014] The third technical solution of the present invention is to provide an application of the above-mentioned CoNiFe-LDH / NF nanowire electrode in the field of lignin-based fuel cells.

[0015] Technical solution four of the present invention: provides a lignin-based fuel cell, which comprises an anolyte, a catholyte, a cathode electrode and an anode electrode; the anolyte is prepared by dissolving lignin in an alkaline solution; the cathode electrolyte is prepared by dissolving a pentavalent vanadium salt and a cathode regeneration oxidant in an acid solution; the cathode electrode is a graphite felt electrode; and the anode electrode is the above-mentioned CoNiFe-LDH / NF nanowire electrode.

[0016] Preferably, the lignin is one or more of enzymatic lignin, prehydrolyzed lignin, sodium lignin sulfonate and alkali lignin; the pentavalent vanadium salt is vanadium pentoxide, vanadium oxysulfate or vanadium nitrate; the cathode regeneration oxidant is one or more of nitric acid, oxygen, hydrogen peroxide and potassium permanganate; the hydroxide ion concentration of the alkali in the anode electrolyte is 0.05-5.0 mol / L, and the content of lignin molecules is 1-100 g / L; the concentration of the pentavalent vanadium salt in the cathode electrolyte is 0.05-5 mol / L; the operating temperature of the lignin-based fuel cell is 10-120°C.

[0017] The present invention requires that the lignin-based fuel cell be preheated to 10-120° C. before being operated.

[0018] Preferably, the alkali in the alkali solution is one or more of KOH, NaOH and ammonia water.

[0019] Preferably, the acid in the acid solution is one or more of hydrochloric acid, sulfuric acid and nitric acid; and the concentration of the acid in the cathode electrolyte is 0.05 to 8 mol / L.

[0020] Preferably, a peristaltic pump is used to pass the cathode electrolyte and the anode electrolyte to the cathode chamber and the anode chamber of the lignin-based fuel cell respectively, so that the lignin-based fuel cell is operated to depolymerize lignin while generating electricity.

[0021] More preferably, the hydroxide ion concentration of the alkali in the anolyte is 0.1 to 3 mol / L, most preferably 1 to 2 mol / L.

[0022] More preferably, the content of lignin molecules in the anolyte is 5 to 70 g / L, most preferably 20 to 50 g / L.

[0023] Preferably, when the cathode regeneration oxidant is nitric acid, the added amount is 0.01 to 8 mol / L; when the cathode regeneration oxidant is oxygen, the oxygen introduction rate is 1 to 100 mL / min.

[0024] The fifth technical solution of the present invention is to provide a method for co-production and utilization of the anode electrolyte in the above-mentioned lignin-based fuel cell, comprising the following steps:

[0025] The lignin in the anode electrolyte is directionally depolymerized through an electrolysis reaction of a lignin-based fuel cell, and then aviation fuel components are co-produced.

[0026] The directional depolymerization is directional depolymerization until the molar concentration of C8-C16 components in the anode electrolyte reaches 5-30%.

[0027] Preferably, the method for co-producing aviation fuel components comprises the following steps: extracting the electrolyte obtained after directional depolymerization with ethyl acetate, then heating and evaporating to remove the ethyl acetate to obtain an aviation fuel precursor; mixing the aviation fuel precursor with a catalyst and a solvent, and performing a hydrodeoxygenation treatment to obtain the aviation fuel component.

[0028] Preferably, the solvent is cyclohexane, n-octane or n-dodecane.

[0029] Preferably, the catalyst is one or more of a Pt-based catalyst, a Ni-based catalyst and a Pd-based catalyst; the hydrogen pressure of the hydrodeoxygenation treatment is 2 to 5 MPa, the heating temperature is 80 to 400° C., and the reaction time is 5 to 12 h.

[0030] More preferably, the hydrogen pressure of the hydrodeoxygenation treatment is 3-4 MPa, the heating temperature is 150-250° C., and the reaction time is 6-8 h.

[0031] The beneficial technical effects of the present invention are as follows:

[0032] The present invention adopts CoNiFe-LDH / NF nanowire electrodes prepared by cheap and environmentally friendly transition metals to construct a high-performance lignin-based fuel cell and simultaneously directionally depolymerize lignin, which can produce aviation fuel precursors (C8-C16 aromatic compounds) while producing clean electricity, and further produce aviation fuel components through hydrogenation and deoxygenation, thereby achieving the dual purposes of power generation and preparation of aviation fuel components, and has good application value.

[0033] The present invention grows CoNiFe-LDH nanowires on the surface of nickel foam by a hydrothermal method to prepare a CoNiFe-LDH / NF nanowire electrode, which has the advantages of large specific surface area, high catalytic activity, excellent electrocatalytic activity, simple preparation process, etc. It is used as an electrocatalyst to improve the electron transfer rate and the specific surface area of ​​the electrochemical reaction. The lignin-based fuel cell prepared by this electrode has better lignin degradation activity, can induce lignin macromolecules to efficiently and directional depolymerize into aviation fuel precursors, thereby improving the various performances and product selectivity of the lignin-based fuel cell; the aviation fuel precursor produced by co-production can be used to prepare aviation fuel components by hydrogenation and deoxygenation. The lignin-based fuel cell prepared by the present invention has excellent battery power density and open circuit voltage, can achieve efficient conversion from biomass energy to electrical energy, and can co-produce aviation fuel components.

[0034] The anode electrolyte used in the lignin-based fuel cell of the present invention does not require the introduction of external redox couples to assist the transmission of electrons, which simplifies the process of electron transfer and separation and purification of degraded lignin. The electrolyte does not need to be pre-degraded and can be used for direct power generation, thus avoiding the condensation of lignin, simplifying the power generation process and reducing energy consumption.

[0035] The lignin-based fuel cell of the present invention generates electricity by directly electrocatalytically oxidizing lignin on the electrode, does not require the introduction of external conditions such as microorganisms, is not easily disturbed by other factors, and has high operating stability of the fuel cell. The application of modified electrodes can greatly increase the lignin oxidation rate and electron transfer rate, thereby greatly improving the performance of the fuel cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0037] Figure 1 This is a current density-voltage-output power diagram of the lignin-based fuel cell prepared in Example 1-2.

[0038] Figure 2 1 and 2 are XRD patterns of the CoNi-LDH / NF nanowire electrode in Example 1 and the CoNiFe-LDH / NF nanowire electrode in Example 2.

[0039] Figure 3 These are SEM images of the CoNi-LDH / NF nanowire electrode in Example 1 at different magnifications.

[0040] Figure 4 These are SEM images of the CoNiFe-LDH / NF nanowire electrode in Example 2 at different magnifications.

[0041] Figure 5 This is a current density-voltage-output power diagram of the lignin-based fuel cell prepared in Example 3.

[0042] Figure 6 This is a current density-voltage-output power diagram of the lignin-based fuel cell prepared in Example 4.

[0043] Figure 7 This is a graph of the long-term continuous power generation of the lignin-based fuel cell prepared in Example 5.

[0044] Figure 8 This is the GC-MS graph of the extract in effect verification 1. Wherein, a is the type of compound, and b is the mass spectrum of the corresponding compound.

[0045] Fig. 9 This is the current density-voltage-output power diagram of the lignin-based fuel cell prepared in Comparative Example 1.

[0046] Fig.10 This is the current density-voltage-output power diagram of the lignin-based fuel cell prepared in Comparative Example 3. DETAILED DESCRIPTION

[0047] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0048] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0049] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.

[0050] The words “include,” “including,” “have,” “contain,” etc. used in the present invention are open-ended terms, meaning including but not limited to.

[0051] The "room temperature" in the present invention is 10-30°C unless otherwise specified.

[0052] The enzymatic lignin used in the following examples and comparative examples of the present invention was purchased from Shandong Longli Biotechnology Co., Ltd. Nickel foam was purchased from Lige Technology Co., Ltd. and was ultrasonically cleaned in anhydrous ethanol, acetone, HCl and deionized water before use. Graphite felt was purchased from Taiwan Carbon Energy, China, and was calcined before use to remove surface organic matter. The calcination temperature was 420°C, the calcination time was 4h, and the heating rate was 5°C / min. Pt / C catalyst was purchased from Shanghai McLean Biochemical Technology Co., Ltd.

[0053] The electrical properties (current density, voltage, output power) of the battery prepared by the present invention were tested using a scanning current method.

[0054] All raw materials used in the following examples and comparative examples of the present invention are commercially available products.

[0055] Example 1

[0056] A method for preparing a lignin-based fuel cell, comprising the following steps:

[0057] 1. Preparation of CoNi-LDH / NF nanowire electrode: 2 mmol Co(NO 3 ) 2 6H 2 O, 1mmol NiCl 2 6H 2 O, 5mmol NH 4 F. 5 mmol urea was dissolved in 50 mL deionized water, and then 4 cm × 1 cm × 0.7 cm nickel foam was added for impregnation, and then placed in a high-pressure reactor for hydrothermal reaction at 140 ° C for 6 h. After the reaction, the sample was taken out, washed with deionized water, and dried to obtain a CoNi-LDH / NF nanowire electrode.

[0058] 2. Preparation of anolyte: Weigh 5.61 g KOH and dissolve it in 50 mL deionized water. Then weigh 2 g enzymatic lignin and add it to the solution. Stir for 10 min and filter to obtain the anolyte.

[0059] 3. Preparation of cathode electrolyte: Weigh 20 g of vanadium pentoxide powder and add it to a beaker containing 524 mL of deionized water, and stir at room temperature. Then take 76 mL of concentrated sulfuric acid (mass fraction 98.3%) and slowly add it to the solution; then add 4 mL of nitric acid (mass fraction 68%), and continue stirring the solution until a bright yellow clear solution is formed. Then let it stand for 24 hours, and measure 100 mL as the cathode electrolyte.

[0060] 4. Preparation of lignin-based fuel cells: The prepared CoNi-LDH / NF nanowire electrode was cut into 4cm×0.25cm×0.7cm, and then the CoNi-LDH / NF nanowire electrode was used as the anode electrode in the S-shaped flow channel in the anode graphite plate, and the graphite felt was filled in the S-shaped flow channel in the cathode graphite plate as the cathode electrode; then the battery was assembled in the order of metal cover plate, anode graphite plate, polytetraethylene film, Nafion211 membrane, polytetrafluoroethylene film, cathode graphite plate containing graphite felt, and metal cover plate through the graphite plate, load (LED lamp) wire, fixed end plate, etc., and the battery and the load were connected with wires. Then the above-mentioned anode electrolyte was added to the anode electrolyte tank through a peristaltic pump, and the cathode electrolyte was added to the cathode electrolyte tank. The anode electrolyte tank was connected to the anode inlet and outlet of the battery with a pipe, and the cathode tank was connected to the cathode inlet and outlet of the battery. Oxygen was introduced into the cathode electrolyte tank at a flow rate of 40mL / min, and the battery was operated at 90°C.

[0061] Example 2

[0062] A method for preparing a lignin-based fuel cell, comprising the following steps:

[0063] 1. Preparation of CoNiFe-LDH / NF nanowire electrode: 2 mmol Co(NO 3 ) 2 6H 2 O, 1mmol NiCl 2 6H 2 O, 0.5mmol FeCl 3 6H 2 O, 5mmol NH 4 F. 5 mmol urea was dissolved in 50 mL deionized water, and then 4 cm × 1 cm × 0.7 cm nickel foam was added for impregnation, and then placed in a high-pressure reactor for hydrothermal reaction at 140 ° C for 6 h. After the reaction, the sample was taken out, washed with deionized water, and dried to obtain a CoNiFe-LDH / NF nanowire electrode.

[0064] 2. Preparation of anolyte: Weigh 5.61 g KOH and dissolve it in 50 mL deionized water. Then weigh 2 g enzymatic lignin and add it to the solution. Stir for 10 min and filter to obtain the anolyte.

[0065] 3. Preparation of cathode electrolyte: Weigh 20 g of vanadium pentoxide powder and add it to a beaker containing 524 mL of deionized water, and stir at room temperature. Then take 76 mL of concentrated sulfuric acid (mass fraction 98.3%) and slowly add it to the solution; then add 4 mL of nitric acid (mass fraction 68%), and continue stirring the solution until a bright yellow clear solution is formed. Then let it stand for 24 hours, and measure 100 mL as the cathode electrolyte.

[0066] 4. Preparation of lignin-based fuel cells: The prepared CoNiFe-LDH / NF nanowire electrode is cut into 4cm×0.25cm×0.7cm, and then the CoNiFe-LDH / NF nanowire electrode is used as the anode electrode in the S-shaped flow channel in the anode graphite plate, and the graphite felt is filled in the S-shaped flow channel in the cathode graphite plate as the cathode electrode; then the battery is assembled in the order of metal cover plate, anode graphite plate, polytetraethylene film, Nafion211 membrane, polytetrafluoroethylene film, cathode graphite plate containing graphite felt, and metal cover plate through the graphite plate, load (LED lamp) wire, fixed end plate, etc., and the battery and the load are connected with wires. Then the above-mentioned anode electrolyte is added to the anode electrolyte tank through a peristaltic pump, and the cathode electrolyte is added to the cathode electrolyte tank. The anode electrolyte tank is connected to the anode inlet and outlet of the battery with a pipe, and the cathode tank is connected to the cathode inlet and outlet of the battery. Oxygen was introduced into the cathode electrolyte tank at a flow rate of 40 mL / min, and the cell was operated at 90°C.

[0067] Figure 1 This is a current density-voltage-output power diagram of the lignin-based fuel cell prepared in Example 1-2.

[0068] Figure 1 In the figure, CoNiFe-LDH represents Example 2, and CoNi-LDH represents Example 1.

[0069] like Figure 1 As shown in Figure 1, the maximum voltage of the lignin-based fuel cell prepared in Example 1 is 1.60 V, and the maximum current density is 1323.7 mA / cm 2 , the maximum power density is 227.93mW / cm 2 The maximum voltage of the lignin-based fuel cell prepared in Example 2 is 1.65 V, and the maximum current density is 1794.4 mA / cm 2 , the maximum power density is 282.49mW / cm 2 The battery performance of Example 2 is significantly better than that of Example 1, indicating that iron doping can effectively increase the electron transfer rate.

[0070] Figure 2 1 and 2 are XRD patterns of the CoNi-LDH / NF nanowire electrode in Example 1 and the CoNiFe-LDH / NF nanowire electrode in Example 2.

[0071] In the figure, CoNi-LDH represents Example 1, and CoNiFe-LDH represents Example 2.

[0072] like Figure 2As shown, CoNi-LDH before iron doping exhibits a cobalt hydroxide peak, while a new nickel hydroxide peak appears after iron doping, indicating that the doping of iron ions significantly changes the coordination structure of the catalyst.

[0073] Figure 3 These are SEM images of the CoNi-LDH / NF nanowire electrode in Example 1 at different magnifications.

[0074] Figure 4 These are SEM images of the CoNiFe-LDH / NF nanowire electrode in Example 2 at different magnifications.

[0075] like Figure 3-4 As shown, the morphology of the original CoNi-LDH is partially granular and nanowire-like, while after iron doping, it presents a uniform nanowire shape, indicating that iron doping promotes the formation of nanowires and greatly increases the electrochemical active surface area.

[0076] Example 3 (only the operating temperature of step 4 is modified to 25°C)

[0077] A method for preparing a lignin-based fuel cell, comprising the following steps:

[0078] 1. Preparation of CoNiFe-LDH / NF nanowire electrode: 2 mmol Co(NO 3 ) 2 6H 2 O, 1mmol NiCl 2 6H 2 O, 0.5mmol FeCl 3 6H 2 O, 5mmol NH 4 F. 5 mmol urea was dissolved in 50 mL deionized water, and then 4 cm × 1 cm × 0.7 cm nickel foam was added for impregnation, and then placed in a high-pressure reactor for hydrothermal reaction at 140 ° C for 6 h. After the reaction, the sample was taken out, washed with deionized water, and dried to obtain a CoNiFe-LDH / NF nanowire electrode.

[0079] 2. Preparation of anolyte: Weigh 5.61 g KOH and dissolve it in 50 mL deionized water. Then weigh 2 g enzymatic lignin and add it to the solution. Stir for 10 min and filter to obtain the anolyte.

[0080] 3. Preparation of cathode electrolyte: Weigh 20 g of vanadium pentoxide powder and add it to a beaker containing 524 mL of deionized water, and stir at room temperature. Then take 76 mL of concentrated sulfuric acid (mass fraction 98.3%) and slowly add it to the solution; then add 4 mL of nitric acid (mass fraction 68%), and continue stirring the solution until a bright yellow clear solution is formed. Then let it stand for 24 hours, and measure 100 mL as the cathode electrolyte.

[0081] 4. Preparation of lignin-based fuel cells: The prepared CoNiFe-LDH / NF nanowire electrode is cut into 4cm×0.25cm×0.7cm, and then the CoNiFe-LDH / NF nanowire electrode is used as the anode electrode in the S-shaped flow channel in the anode graphite plate, and the graphite felt is filled in the S-shaped flow channel in the cathode graphite plate as the cathode electrode; then the battery is assembled in the order of metal cover plate, anode graphite plate, polytetraethylene film, Nafion211 membrane, polytetrafluoroethylene film, cathode graphite plate containing graphite felt, and metal cover plate through the graphite plate, load (LED lamp) wire, fixed end plate, etc., and the battery and the load are connected with wires. Then the above-mentioned anode electrolyte is added to the anode electrolyte tank through a peristaltic pump, and the cathode electrolyte is added to the cathode electrolyte tank. The anode electrolyte tank is connected to the anode inlet and outlet of the battery with a pipe, and the cathode tank is connected to the cathode inlet and outlet of the battery. Oxygen was introduced into the cathode electrolyte tank at a flow rate of 40 mL / min, and the cell was operated at 25°C.

[0082] Figure 5 This is a current density-voltage-output power diagram of the lignin-based fuel cell prepared in Example 3.

[0083] like Figure 5 As shown in Figure 3, the maximum voltage of the lignin-based fuel cell prepared in Example 3 is 1.30 V, and the maximum current density is 553.17 mA / cm 2 , the maximum power density is 73.89mW / cm 2 , the battery performance is lower than that of Example 2, but the room temperature power generation process is more energy-efficient.

[0084] Example 4 (Only replacing enzymatic lignin with alkali lignin)

[0085] A method for preparing a lignin-based fuel cell, comprising the following steps:

[0086] 1. Preparation of CoNiFe-LDH / NF nanowire electrode: 2 mmol Co(NO 3 ) 2 6H 2 O, 1mmol NiCl 2 6H 2 O, 0.5mmol FeCl 3 6H2 O, 5mmol NH 4 F. 5 mmol urea was dissolved in 50 mL deionized water, and then 4 cm × 1 cm × 0.7 cm nickel foam was added for impregnation, and then placed in a high-pressure reactor for hydrothermal reaction at 140 ° C for 6 h. After the reaction, the sample was taken out, washed with deionized water, and dried to obtain a CoNiFe-LDH / NF nanowire electrode.

[0087] 2. Preparation of anolyte: Weigh 5.61 g KOH and dissolve it in 50 mL deionized water. Then weigh 2 g alkali lignin and add it to the solution. Stir for 10 min and filter to obtain the anolyte.

[0088] 3. Preparation of cathode electrolyte: Weigh 20 g of vanadium pentoxide powder and add it to a beaker containing 524 mL of deionized water, and stir at room temperature. Then take 76 mL of concentrated sulfuric acid (mass fraction 98.3%) and slowly add it to the solution; then add 4 mL of nitric acid (mass fraction 68%), and continue stirring the solution until a bright yellow clear solution is formed. Then let it stand for 24 hours, and measure 100 mL as the cathode electrolyte.

[0089] 4. Preparation of lignin-based fuel cells: The prepared CoNiFe-LDH / NF nanowire electrode is cut into 4cm×0.25cm×0.7cm, and then the CoNiFe-LDH / NF nanowire electrode is used as the anode electrode in the S-shaped flow channel in the anode graphite plate, and the graphite felt is filled in the S-shaped flow channel in the cathode graphite plate as the cathode electrode; then the battery is assembled in the order of metal cover plate, anode graphite plate, polytetraethylene film, Nafion211 membrane, polytetrafluoroethylene film, cathode graphite plate containing graphite felt, and metal cover plate through the graphite plate, load (LED lamp) wire, fixed end plate, etc., and the battery and the load are connected with wires. Then the above-mentioned anode electrolyte is added to the anode electrolyte tank through a peristaltic pump, and the cathode electrolyte is added to the cathode electrolyte tank. The anode electrolyte tank is connected to the anode inlet and outlet of the battery with a pipe, and the cathode tank is connected to the cathode inlet and outlet of the battery. Oxygen was introduced into the cathode electrolyte tank at a flow rate of 40 mL / min, and the cell was operated at 90°C.

[0090] Figure 6 This is a current density-voltage-output power diagram of the lignin-based fuel cell prepared in Example 4.

[0091] like Figure 6 As shown in Figure 4, the maximum voltage of the lignin-based fuel cell prepared in Example 4 is 1.32 V, and the maximum current density is 623.09 mA / cm 2 , the maximum power density is 169.20mW / cm 2The battery performance is lower than that of Example 2, indicating that the performance of using enzymatic lignin to generate electricity is higher than that of using alkaline lignin.

[0092] Example 5 (only the amount of enzymatic lignin added was modified to 1 g)

[0093] A method for preparing a lignin-based fuel cell, comprising the following steps:

[0094] 1. Preparation of CoNiFe-LDH / NF nanowire electrode: 2 mmol Co(NO 3 ) 2 6H 2 O, 1mmol NiCl 2 6H 2 O, 0.5mmol FeCl 3 6H 2 O, 5mmol NH 4 F. 5 mmol urea was dissolved in 50 mL deionized water, and then 4 cm × 1 cm × 0.7 cm nickel foam was added for impregnation, and then placed in a high-pressure reactor for hydrothermal reaction at 140 ° C for 6 h. After the reaction, the sample was taken out, washed with deionized water, and dried to obtain a CoNiFe-LDH / NF nanowire electrode.

[0095] 2. Preparation of anolyte: Weigh 5.61 g KOH and dissolve it in 50 mL deionized water. Then weigh 1 g enzymatic lignin and add it to the solution. Stir for 10 min and filter to obtain the anolyte.

[0096] 3. Preparation of cathode electrolyte: Weigh 20 g of vanadium pentoxide powder and add it to a beaker containing 524 mL of deionized water, and stir at room temperature. Then take 76 mL of concentrated sulfuric acid (mass fraction 98.3%) and slowly add it to the solution; then add 4 mL of nitric acid (mass fraction 68%), and continue stirring the solution until a bright yellow clear solution is formed. Then let it stand for 24 hours, and measure 100 mL as the cathode electrolyte.

[0097] 4. Preparation of lignin-based fuel cells: The prepared CoNiFe-LDH / NF nanowire electrode is cut into 4cm×0.25cm×0.7cm, and then the CoNiFe-LDH / NF nanowire electrode is used as the anode electrode in the S-shaped flow channel in the anode graphite plate, and the graphite felt is filled in the S-shaped flow channel in the cathode graphite plate as the cathode electrode; then the battery is assembled in the order of metal cover plate, anode graphite plate, polytetraethylene film, Nafion211 membrane, polytetrafluoroethylene film, cathode graphite plate containing graphite felt, and metal cover plate through the graphite plate, load (LED lamp) wire, fixed end plate, etc., and the battery and the load are connected with wires. Then the above-mentioned anode electrolyte is added to the anode electrolyte tank through a peristaltic pump, and the cathode electrolyte is added to the cathode electrolyte tank. The anode electrolyte tank is connected to the anode inlet and outlet of the battery with a pipe, and the cathode tank is connected to the cathode inlet and outlet of the battery. Oxygen was introduced into the cathode electrolyte tank at a flow rate of 40 mL / min, and the cell was operated at 90°C.

[0098] Effect verification 1

[0099] The lignin-based fuel cell prepared in Example 5 was subjected to a long-term continuous discharge test at a voltage of 0.3 V to detect the corresponding battery performance. The test results are as follows: Figure 7 shown.

[0100] The lignin-based fuel cell prepared in Example 5 was subjected to a long-term continuous discharge test at a voltage of 0.3 V. During the long-term continuous discharge test, when the molar concentration of the C8-C16 component in the anolyte was detected to reach 20%, power generation was stopped, and the obtained anolyte was extracted with ethyl acetate. The obtained extract was the co-produced aviation fuel precursor component, and the types of compounds in the extract were detected. The test results are shown in FIG. Figure 8 shown.

[0101] Figure 7 This is a graph of the long-term continuous power generation of the lignin-based fuel cell prepared in Example 5.

[0102] like Figure 7 As shown, at a voltage of 0.3 V, 1 g of enzymatically hydrolyzed lignin can generate 529 mWh of electricity.

[0103] Figure 8 This is the GC-MS graph of the extract in effect verification 1. Wherein, a is the type of compound, and b is the mass spectrum of the corresponding compound.

[0104] Figure 8 The results show that after the electrolyte produced by power generation is extracted with ethyl acetate, various aviation fuel precursor components such as benzoic acid, benzaldehyde, and acetophenone compounds can be obtained.

[0105] Example 6

[0106] A method for preparing aviation fuel components using an aviation fuel precursor solution produced by power generation and cogeneration, comprising the following steps:

[0107] The extract in effect verification 1 was heated to evaporate the solvent to obtain a solid lignin degradation product; 0.01g of lignin degradation product, 0.05g of Pt / C catalyst powder and 10mL of cyclohexane solvent were added to the autoclave, and after removing the air from the autoclave, 5MPa of high-pressure hydrogen was filled in, and the product yield was detected by gas chromatography after heating and stirring at 180°C for 8h. Hexane was used as the internal standard, and the conversion rate, yield and selectivity were calculated by the internal standard method. The calculation formula is as follows:

[0108]

[0109] Among them, f i and f s are the correction factors for the analyte and internal standard, respectively, calculated using the effective carbon number method. i and A s are the peak areas of the analyte and internal standard, m s is the mass of the internal standard, m i The results show that the yield of aviation fuel components is about 21.3% and the conversion rate is about 65%.

[0110] Comparative Example 1 (Nickel foam as anode electrode)

[0111] A method for preparing a lignin-based fuel cell, comprising the following steps:

[0112] 1. Preparation of anolyte: Weigh 5.61 g KOH and dissolve it in 50 mL deionized water. Then weigh 2 g enzymatic lignin and add it to the solution. Stir for 10 min and filter to obtain anolyte.

[0113] 2. Preparation of cathode electrolyte: Weigh 20 g of vanadium pentoxide powder and add it to a beaker containing 524 mL of deionized water, and stir at room temperature. Then take 76 mL of concentrated sulfuric acid (mass fraction 98.3%) and slowly add it to the solution; then add 4 mL of nitric acid (mass fraction 68%), and continue stirring the solution until a bright yellow clear solution is formed. Then let it stand for 24 hours, and measure 100 mL as the cathode electrolyte.

[0114] 3. Preparation of lignin-based fuel cells: Cut nickel foam into 4cm×0.25cm×0.7cm, then use nickel foam as the anode electrode in the S-shaped flow channel in the anode graphite plate, and fill the S-shaped flow channel in the cathode graphite plate with graphite felt as the cathode electrode; then assemble the battery in the order of metal cover plate, anode graphite plate, polytetraethylene film, Nafion211 membrane, polytetrafluoroethylene film, cathode graphite plate containing graphite felt, and metal cover plate through graphite plate, load (LED lamp) wire, fixed end plate, etc., and connect the battery and load with wires. Then add the above-mentioned anode electrolyte to the anode electrolyte tank through a peristaltic pump, and add the cathode electrolyte to the cathode electrolyte tank. Use a pipe to connect the anode electrolyte tank to the anode inlet and outlet of the battery, and the cathode tank to the cathode inlet and outlet of the battery. Oxygen is passed into the cathode electrolyte tank at a flow rate of 40mL / min, and the battery is operated at 90°C.

[0115] Fig. 9 This is the current density-voltage-output power diagram of the lignin-based fuel cell prepared in Comparative Example 1.

[0116] like Fig. 9 As shown in Figure 1, the maximum voltage of the lignin-based fuel cell prepared in Comparative Example 1 is 1.56 V, and the maximum current density is 1268.6 mA / cm 2 , the maximum power density is 223.43mW / cm 2 The performance is not as good as the CoNiFe-LDH / NF nanowire electrode in Example 2, so the use of CoNiFe-LDH / NF nanowire electrode can achieve more efficient degradation of lignin and coupled power generation.

[0117] Comparative Example 2 (graphite felt as anode electrode)

[0118] A method for preparing a lignin-based fuel cell, comprising the following steps:

[0119] 1. Preparation of anolyte: Weigh 2g NaOH and dissolve it in 50mL deionized water. Then weigh 1g enzymatic lignin and add it to the solution. Stir for 10min and filter to obtain anolyte.

[0120] 2. Preparation of cathode electrolyte: Weigh 20 g of vanadium pentoxide powder and add it to a beaker containing 524 mL of deionized water, and stir at room temperature. Then take 76 mL of concentrated sulfuric acid (mass fraction 98.3%) and slowly add it to the solution; then add 4 mL of nitric acid (mass fraction 68%), and continue stirring the solution until a bright yellow clear solution is formed. Then let it stand for 24 hours, and measure 100 mL as the cathode electrolyte.

[0121] 3. Preparation of lignin-based fuel cells: Graphite felt is filled in the S-shaped flow channel in the anode graphite plate as the anode electrode, and graphite felt is filled in the S-shaped flow channel in the cathode graphite plate as the cathode electrode; then the battery is assembled in the order of metal cover plate, anode graphite plate, polytetraethylene film, Nafion211 membrane, polytetrafluoroethylene film, cathode graphite plate containing graphite felt, and metal cover plate through graphite plate, load (LED lamp) wire, fixed end plate, etc., and the battery and load are connected with wires. Then the above-mentioned anode electrolyte is added to the anode electrolyte tank through a peristaltic pump, and the cathode electrolyte is added to the cathode electrolyte tank. The anode electrolyte tank is connected to the anode inlet and outlet of the battery with a pipe, and the cathode tank is connected to the cathode inlet and outlet of the battery. Oxygen is passed into the cathode electrolyte tank at a flow rate of 40mL / min, and the battery is operated at 90°C.

[0122] The maximum voltage of the lignin-based fuel cell prepared in Comparative Example 2 was 1.45 V, and the maximum current density was 397.44 mA / cm 2 , the maximum power density is 108.54mW / cm 2 The performance is not as good as the CoNiFe-LDH / NF nanowire electrode in Example 2, so the use of CoNiFe-LDH / NF nanowire electrode can achieve more efficient degradation of lignin and coupled power generation.

[0123] Comparative Example 3 (Only modifying the anode material)

[0124] A method for preparing a lignin-based fuel cell, comprising the following steps:

[0125] 1. Preparation of sulfur-doped CoNi-LDH / GF electrode: 3.75 mmol Co(NO 3 ) 2 6H 2 O, 3.75mmol Ni(CH 3 COO 2 ·4H 2 O, 10 mmol NH 4 F. 25mmol urea was dissolved in 70mL deionized water, added to 5cm×0.5cm×0.5cm graphite felt for impregnation, and placed in a high-pressure reactor for hydrothermal reaction at 120℃ for 5h. After the reaction, the sample was taken out, washed with deionized water, and dried to obtain CoNi-LDH / GF. Then 0.75mmol C 2 H 5 NS (thioacetamide) was dissolved in 50 mL of ethylene glycol, and CoNi-LDH / GF was added for impregnation, and then placed in a high-pressure reactor for hydrothermal reaction at 120°C for 2.5 h. After the reaction, the sample was taken out, washed with deionized water, and dried to obtain a CoNi-LDH-S / GF electrode.

[0126] 2. Preparation of anolyte: Weigh 5.61 g KOH and dissolve it in 50 mL deionized water. Then weigh 2 g enzymatic lignin and add it to the solution. Stir for 10 min and filter to obtain the anolyte.

[0127] 3. Preparation of cathode electrolyte: Weigh 20 g of vanadium pentoxide powder and add it to a beaker containing 524 mL of deionized water, and stir at room temperature. Then take 76 mL of concentrated sulfuric acid (mass fraction 98.3%) and slowly add it to the solution; then add 4 mL of nitric acid (mass fraction 68%), and continue stirring the solution until a bright yellow clear solution is formed. Then let it stand for 24 hours, and measure 100 mL as the cathode electrolyte.

[0128] 4. Preparation of lignin-based fuel cells: CoNi-LDH-S / GF electrode is used as the anode electrode in the S-shaped flow channel in the anode graphite plate, and graphite felt is filled in the S-shaped flow channel in the cathode graphite plate as the cathode electrode; then the battery is assembled in the order of metal cover plate, anode graphite plate, polytetraethylene film, Nafion211 membrane, polytetrafluoroethylene film, cathode graphite plate containing graphite felt, and metal cover plate through graphite plate, load (LED lamp) wire, fixed end plate, etc., and the battery and load are connected with wires. Then the above-mentioned anode electrolyte is added to the anode electrolyte tank through a peristaltic pump, and the cathode electrolyte is added to the cathode electrolyte tank. The anode electrolyte tank is connected to the anode inlet and outlet of the battery with a pipe, and the cathode tank is connected to the cathode inlet and outlet of the battery. Oxygen is passed into the cathode electrolyte tank at a flow rate of 40mL / min, and the battery is operated at 90°C.

[0129] Fig.10 This is the current density-voltage-output power diagram of the lignin-based fuel cell prepared in Comparative Example 3.

[0130] Depend on Fig.10 It can be seen that the maximum voltage of the lignin-based fuel cell prepared in Comparative Example 3 is 1.69 V, and the maximum current density is 831.76 mA / cm 2 , the maximum power density is 234.90mW / cm 2 The performance is not as good as the CoNiFe-LDH / NF nanowire electrode in Example 2. In comparison, the CoNiFe-LDH / NF nanowire electrode can achieve more efficient degradation of lignin and coupled power generation. In addition, in the subsequent hydrodeoxygenation step, the platinum-based catalyst will be poisoned when it encounters a compound system containing the S element, causing the catalyst to lose its catalytic activity, so it is not suitable to use a sulfur-containing electrocatalyst.

[0131] Comparative Example 4 (Only modifying the anode material)

[0132] A method for preparing a lignin-based fuel cell, comprising the following steps:

[0133] 1. Preparation of CoNiFe-LDH / CoNiFeS electrode: 0.58 g Co(NO 3 ) 2 6H 2 O and 1.3 g 2-methylimidazole were dissolved in 40 mL deionized water, stirred for 10 min and mixed, and a 1 cm × 2 cm carbon cloth was placed in the mixed solution. After standing for 4 h at room temperature, it was rinsed with deionized water and dried to obtain a sample Co-MOF. 3 ) 3 9H 2 O, 0.56 g Ni(NO 3 ) 2 6H 2 O, 0.15 g NH 4 F and 0.61g urea were dissolved in 40mL deionized water. After dissolution, Co-MOF was immersed in the mixed solution and transferred to a 100mL polytetrafluoroethylene-lined stainless steel autoclave, hydrothermal at 140°C for 4h, and the sample was taken out after natural cooling to room temperature, rinsed with deionized water, and dried overnight at 60°C in a vacuum drying oven to obtain CoNiFe-LDH. 50mg thioacetamide was dissolved in 40mL anhydrous ethanol. After stirring evenly, the ethanol solution of thioacetamide and CoNiFe-LDH were transferred to a 100mL polytetrafluoroethylene-lined stainless steel autoclave and hydrothermal at 100°C for 4h. After natural cooling to room temperature, it was rinsed with deionized water and dried to obtain CoNiFe-LDH / CoNiFeS.

[0134] 2. Preparation of anolyte: Weigh 5.61 g KOH and dissolve it in 50 mL deionized water. Then weigh 2 g enzymatic lignin and add it to the solution. Stir for 10 min and filter to obtain the anolyte.

[0135] 3. Preparation of cathode electrolyte: Weigh 20 g of vanadium pentoxide powder and add it to a beaker containing 524 mL of deionized water, and stir at room temperature. Then take 76 mL of concentrated sulfuric acid (mass fraction 98.3%) and slowly add it to the solution; then add 4 mL of nitric acid (mass fraction 68%), and continue stirring the solution until a bright yellow clear solution is formed. Then let it stand for 24 hours, and measure 100 mL as the cathode electrolyte.

[0136] 4. Preparation of lignin-based fuel cells: CoNiFe-LDH / CoNiFeS is used as the anode electrode in the S-shaped flow channel in the anode graphite plate, and graphite felt is filled in the S-shaped flow channel in the cathode graphite plate as the cathode electrode; then the battery is assembled in the order of metal cover plate, anode graphite plate, polytetraethylene film, Nafion211 membrane, polytetrafluoroethylene film, cathode graphite plate containing graphite felt, and metal cover plate through graphite plate, load (LED lamp) wire, fixed end plate, etc., and the battery and load are connected with wires. Then the above-mentioned anode electrolyte is added to the anode electrolyte tank through a peristaltic pump, and the cathode electrolyte is added to the cathode electrolyte tank. The anode electrolyte tank is connected to the anode inlet and outlet of the battery with a pipe, and the cathode tank is connected to the cathode inlet and outlet of the battery. Oxygen is passed into the cathode electrolyte tank at a flow rate of 40mL / min, and the battery is operated at 90°C.

[0137] It was determined that the maximum voltage of the lignin-based fuel cell prepared in Comparative Example 4 was 1.57 V and the maximum current density was 1356.69 mA / cm 2 , the maximum power density is 210.53mW / cm 2 The performance is not as good as the CoNiFe-LDH / NF nanowire electrode in Example 2. In comparison, the CoNiFe-LDH / NF nanowire electrode can achieve more efficient degradation of lignin and coupled power generation. In addition, in the subsequent hydrodeoxygenation step, the platinum-based catalyst will be poisoned when it encounters a compound system containing the S element, causing the catalyst to lose its catalytic activity, so it is not suitable to use a S-containing electrocatalyst.

[0138] Comparative Example 5 (Only modifying the anode material)

[0139] A method for preparing a lignin-based fuel cell, comprising the following steps:

[0140] 1. Preparation of CoNiFe-MOF / LDH electrode: CoCl 2 6H 2 O (300 mg), NiCl 2 6H 2 O (60 mg), FeCl 2 ·4H 2O (30 mg) and urea (380 mg) were mixed in deionized water, and after ultrasonic treatment for 1 h, a 1 cm × 2 cm carbon cloth was placed in the mixed solution, heated at 120 ° C for 12 h, cooled to room temperature, washed with deionized water, and dried at 90 ° C for 12 h to obtain CoNiFe-LDH. CoNiFe-LDH was immersed in 20 mL of N, N-dimethylformamide solution containing 2, 3, 6, 7, 10, 11-hexahydroxytriphenylene benzene, wherein the mass ratio of CoNiFe-LDH to 2, 3, 6, 7, 10, 11-hexahydroxytriphenylene benzene was 1:2. The dispersed solution was sealed in a polytetrafluoroethylene-lined autoclave, hydrothermally reacted at 100 ° C for 24 h, cooled naturally to room temperature, and then thoroughly washed with ultrapure water, N, N-dimethylformamide and ethanol, and dried in a vacuum drying oven at 90 ° C for 12 h to obtain a CoNiFe-MOF / LDH electrode.

[0141] 2. Preparation of anolyte: Weigh 5.61 g KOH and dissolve it in 50 mL deionized water. Then weigh 2 g enzymatic lignin and add it to the solution. Stir for 10 min and filter to obtain the anolyte.

[0142] 3. Preparation of cathode electrolyte: Weigh 20 g of vanadium pentoxide powder and add it to a beaker containing 524 mL of deionized water, and stir at room temperature. Then take 76 mL of concentrated sulfuric acid (mass fraction 98.3%) and slowly add it to the solution; then add 4 mL of nitric acid (mass fraction 68%), and continue stirring the solution until a bright yellow clear solution is formed. Then let it stand for 24 hours, and measure 100 mL as the cathode electrolyte.

[0143] 4. Preparation of lignin-based fuel cells: CoNiFe-MOF / LDH electrode is used as the anode electrode in the S-shaped flow channel in the anode graphite plate, and graphite felt is filled in the S-shaped flow channel in the cathode graphite plate as the cathode electrode; then the battery is assembled in the order of metal cover plate, anode graphite plate, polytetraethylene film, Nafion211 membrane, polytetrafluoroethylene film, cathode graphite plate containing graphite felt, and metal cover plate through graphite plate, load (LED lamp) wire, fixed end plate, etc., and the battery and load are connected with wires. Then the above-mentioned anode electrolyte is added to the anode electrolyte tank through a peristaltic pump, and the cathode electrolyte is added to the cathode electrolyte tank. The anode electrolyte tank is connected to the anode inlet and outlet of the battery with a pipe, and the cathode tank is connected to the cathode inlet and outlet of the battery. Oxygen is passed into the cathode electrolyte tank at a flow rate of 40mL / min, and the battery is operated at 90°C.

[0144] It was determined that the maximum voltage of the lignin-based fuel cell prepared in Comparative Example 5 was 1.56 V and the maximum current density was 1245.14 mA / cm 2, the maximum power density is 246.78mW / cm 2 The performance is not as good as the CoNiFe-LDH / NF nanowire electrode in Example 2, so the use of CoNiFe-LDH / NF nanowire electrode can achieve more efficient degradation of lignin and coupled power generation.

[0145] Comparative Example 6 (Only modifying the anode material)

[0146] A method for preparing a lignin-based fuel cell, comprising the following steps:

[0147] 1. Preparation of nickel foam / manganese cobalt oxide nanowire electrode: 5 mmol Co(NO 3 ) 2 6H 2 O, 2.5mmol Mn(NO 3 ) 2 6H 2 O, 10 mmol NH 4 F. 25mmol urea was dissolved in 70mL deionized water, and 4cm×1cm×0.7cm nickel foam was added for impregnation. The mixture was placed in a high-pressure reactor and hydrothermaled at 120℃ for 5h. After the reaction, the sample was taken out, washed with deionized water, and dried to obtain a nickel foam / manganese cobaltate nanowire electrode.

[0148] 2. Preparation of anolyte: Weigh 5.61 g KOH and dissolve it in 50 mL deionized water. Then weigh 2 g enzymatic lignin and add it to the solution. Stir for 10 min and filter to obtain the anolyte.

[0149] 3. Preparation of cathode electrolyte: Weigh 20 g of vanadium pentoxide powder and add it to a beaker containing 524 mL of deionized water, and stir at room temperature. Then take 76 mL of concentrated sulfuric acid (mass fraction 98.3%) and slowly add it to the solution; then add 4 mL of nitric acid (mass fraction 68%), and continue stirring the solution until a bright yellow clear solution is formed. Then let it stand for 24 hours, and measure 100 mL as the cathode electrolyte.

[0150] 4. Preparation of lignin-based fuel cells: The prepared nickel foam / manganese cobalt oxide nanowire electrode was cut into 4cm×0.25cm×0.7cm, and then the nickel foam / manganese cobalt oxide nanowire electrode was used as the anode electrode in the S-shaped flow channel in the anode graphite plate, and the graphite felt was filled in the S-shaped flow channel in the cathode graphite plate as the cathode electrode; then the battery was assembled in the order of metal cover plate, anode graphite plate, polytetraethylene film, Nafion211 membrane, polytetrafluoroethylene film, cathode graphite plate containing graphite felt, and metal cover plate through the graphite plate, load (LED lamp) wire, fixed end plate, etc., and the battery and the load were connected with wires. Then the above-mentioned anode electrolyte was added to the anode electrolyte tank through a peristaltic pump, and the cathode electrolyte was added to the cathode electrolyte tank. The anode electrolyte tank was connected to the anode inlet and outlet of the battery with a pipe, and the cathode tank was connected to the cathode inlet and outlet of the battery. Oxygen was introduced into the cathode electrolyte tank at a flow rate of 40mL / min, and the battery was operated at 90°C.

[0151] It was determined that the maximum voltage of the lignin-based fuel cell prepared in Comparative Example 6 was 1.60 V and the maximum current density was 796.86 mA / cm 2 , the maximum power density is 191.42mW / cm 2 The performance is not as good as the CoNiFe-LDH / NF nanowire electrode in Example 2, so the use of CoNiFe-LDH / NF nanowire electrode can achieve more efficient degradation of lignin and coupled power generation.

[0152] The above embodiments and comparative examples are comprehensively compared in terms of operating temperature, open circuit voltage, maximum power density, etc. The test results are shown in Table 1.

[0153] Table 1 Comprehensive comparison of lignin-based fuel cell systems

[0154]

[0155] Comparing all the examples and comparative examples, it can be seen that the battery with the best power generation performance is the lignin-based fuel cell system constructed using enzymatic lignin as raw material in Example 2, with an open circuit voltage of 1.65 V and a maximum power density of 282.49 mW / cm 2 , much higher than the control ratio.

[0156] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a CoNiFe-LDH / NF nanowire electrode, characterized in that: The following steps are involved: The Co source, the Ni source, the Fe source, the urea and the ammonium fluoride are dissolved in water to obtain a hydrothermal reaction solution; the foamed nickel is placed in the hydrothermal reaction solution to carry out a hydrothermal reaction to obtain the CoNiFe-LDH / NF nanowire electrode.

2. The preparation method according to claim 1, characterized in that: The Co source is Co(NO3)2; the Ni source is NiCl2; the Fe source is FeCl3; the molar ratio of Co(NO3)2, NiCl2, FeCl3, urea and ammonium fluoride is (1-6):(1-6):(0.2-2):(4-20):(4-20).

3. The preparation method according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 20-200° C., and the time is 1-20 hours.

4. A CoNiFe-LDH / NF nanowire electrode obtained according to the preparation method according to any one of claims 1 to 3.

5. Use of the CoNiFe-LDH / NF nanowire electrode according to claim 4 in the field of lignin-based fuel cells.

6. A lignin-based fuel cell, characterized in that: The lignin-based fuel cell comprises an anolyte, a catholyte, a cathode electrode and an anode electrode; the anolyte is prepared by dissolving lignin in an alkaline solution; the cathode electrolyte is prepared by dissolving a pentavalent vanadium salt and a cathode regeneration oxidant in an acid solution; the cathode electrode is a graphite felt electrode; and the anode electrode is the CoNiFe-LDH / NF nanowire electrode as described in claim 4.

7. The lignin-based fuel cell according to claim 6, characterized in that: The lignin is one or more of enzymatic lignin, prehydrolyzed lignin, sodium lignin sulfonate and alkali lignin; the pentavalent vanadium salt is vanadium pentoxide, vanadium oxysulfate or vanadium nitrate; the cathode regeneration oxidant is one or more of nitric acid, oxygen, hydrogen peroxide and potassium permanganate; the hydroxide ion concentration of the alkali in the anode electrolyte is 0.05-5.0 mol / L, and the content of lignin molecules is 1-100 g / L; the concentration of the pentavalent vanadium salt in the cathode electrolyte is 0.05-5 mol / L; and the operating temperature of the lignin-based fuel cell is 10-120°C.

8. A method for co-production and utilization of anode electrolyte in a lignin-based fuel cell according to claim 6 or 7, characterized in that: The following steps are involved: The lignin in the anode electrolyte is directionally depolymerized through an electrolysis reaction of a lignin-based fuel cell, and then aviation fuel components are co-produced. The directional depolymerization is directional depolymerization until the molar concentration of C8-C16 components in the anode electrolyte reaches 5-30%.

9. The method for co-production and utilization according to claim 8, characterized in that: The method for co-producing aviation fuel components comprises the following steps: extracting the electrolyte obtained after directional depolymerization with ethyl acetate, then heating and evaporating to remove the ethyl acetate to obtain an aviation fuel precursor; mixing the aviation fuel precursor with a catalyst and a solvent, and performing a hydrodeoxygenation treatment to obtain the aviation fuel component.

10. The method for joint production and utilization according to claim 9, characterized in that: The catalyst is one or more of a Pt-based catalyst, a Ni-based catalyst and a Pd-based catalyst; the hydrogen pressure of the hydrodeoxygenation treatment is 2-5 MPa, the heating temperature is 80-400° C., and the reaction time is 5-12 hours.

Citation Information

Patent Citations

  • Method for using lignin for directional synthesis of aviation kerosene aromatic components

    CN105441109A

  • Method for joint production of aromatics and aviation kerosene by using lignin and oils as raw materials

    CN106520169A

  • Difunctional catalytic electrode based on transition metal heterogeneous layered structure and preparation method

    CN113430553A

  • Graphite felt / manganese cobaltate nanowire electrode, preparation method and lignin-based fuel cell

    CN116190683A

  • Method for preparing polycycloalkane aviation kerosene from lignin-derived phenols and formaldehyde

    CN116925804A

Cited By

  • Graphite felt / high-entropy MOF electrode, lignin-based fuel cell and method for co-production of aviation fuel components

    CN120376664A