Method for recycling phenol pollutants in water by using nickel-ruthenium hybrid electrocatalyst

By using nickel-ruthenium hybrid catalyst and electrocatalytic oxidation reaction in industrial wastewater, efficient removal of phenol at room temperature and conversion into high-value chemical phenol quinone is achieved, and the problem of low conversion and yield in the prior art is solved. , reduces energy consumption and carbon emissions, and is suitable for complex water environment treatment.

CN118929857AActive Publication Date: 2024-11-12EAST CHINA NORMAL UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411164572.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

In the prior art, when treating phenol pollutants in industrial wastewater, the conversion rate and yield are relatively low, and there are problems of high energy consumption, high substance consumption and high carbon emissions, making it difficult to selectively convert it into high-value chemicals at room temperature. Benzoquinone.

Method used

A highly active nickel-ruthenium hybrid catalyst was designed and prepared, and a nickel-carbon porous electrode was prepared by electrochemical deposition method of the three-electrode system. The selective conversion of phenol to phenol at room temperature was achieved by combining electrocatalytic oxidation reaction.

Benefits of technology

It achieves efficient removal of phenol from water, improves the yield of p-benzoquinone and the stability of catalysts, avoids the high energy consumption and high carbon emissions of traditional electrocatalytic methods, and is suitable for the treatment of complex water environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929857A_ABST
    Figure CN118929857A_ABST
Patent Text Reader

Abstract

The invention discloses a method for recycling phenol pollutants in water by using a nickel-ruthenium hybrid electrocatalyst, and belongs to the technical field of environmental electrocatalytic water treatment. Aiming at the problems of high energy consumption, high material consumption, high carbon emission and the like of a traditional wastewater treatment mode, the nickel-ruthenium hybrid electrocatalyst loaded on the carbon cloth is prepared by utilizing a simple two-step electrodeposition method. The catalyst has high stability and high selectivity, and can realize directional conversion of phenol pollutants in water to high-value p-benzoquinone under mild conditions, so that removal of the phenol pollutants in water and recovery of high-value-added chemicals are realized at the same time. The invention provides a new method for treatment and resource utilization of the high-concentration phenol wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water treatment, and in particular relates to a method for realizing resource recovery of phenol pollutants in water by utilizing a nickel-ruthenium hybrid electrocatalyst. Background Art

[0002] The continuous development of modern industry has driven the gross domestic product to record highs, but at the same time, the industrial production process has also produced a large amount of toxic and harmful industrial wastewater, and its treatment has become one of the bottlenecks for the sustainable development of modern industry. Among them, high-concentration organic wastewater is the most common type of industrial wastewater. Because it contains many types of organic pollutants, high concentrations, high toxicity, and difficulty in biodegradation, it has posed a serious threat to the ecological environment and human health, and is regarded by all countries as one of the environmental problems that need to be solved urgently. For a long time, the use of chemical oxidation and other technologies to achieve efficient mineralization of organic pollutants in wastewater has been the main strategy to deal with the above problems. However, the traditional wastewater treatment model that only takes the mineralization of toxic organic pollutants as a single goal has limitations such as high energy consumption, high material consumption and high carbon emissions, which is in sharp contradiction with the green, low-carbon and circular development model currently advocated. In order to promote the industrial wastewater treatment process to move towards the goal of reducing pollution and reducing carbon emissions, it is urgent to recycle and utilize high-concentration organic pollutants in industrial wastewater.

[0003] With the rapid development of modern chemical industry, the discharge of phenolic wastewater from industrial sectors such as petrochemical, pharmaceutical, oil refining, papermaking, phenolic resin and coking has increased dramatically. Phenolic wastewater poses a serious threat to the ecological environment and human health, so it must be treated to meet relevant emission standards. In phenolic wastewater, phenol is usually the most important pollutant, and its concentration can be as high as hundreds or even tens of thousands of milligrams per liter. Therefore, the recovery of phenol in wastewater is of great reference significance for the development of a sustainable society. p-Benzoquinone, as a common intermediate product in the degradation process of phenols, is usually regarded as a by-product due to its extremely low yield. In fact, p-Benzoquinone is not only an important chemical raw material for industrial products such as fungicides and dyes, but also a potential electrode material for lithium-ion batteries due to its high theoretical specific capacity and voltage. These demands make the economic value of p-Benzoquinone (~100,000 yuan / ton) significantly higher than that of phenol (~5,000 yuan / ton) in the market. In view of this, the selective conversion of phenol pollutants in wastewater into p-Benzoquinone can simultaneously achieve the removal of phenol pollutants and the recovery of high-value chemicals.

[0004] Electrocatalytic synthesis technology cleverly combines electrochemistry and organic synthesis processes, and can construct specific chemical bonds in a simple, efficient and controllable manner. This technology uses electrons as reagents and realizes the redox reaction of organic compounds to generate target products through electron gain and loss. It is regarded as a representative of "green and sustainable" chemistry. So far, researchers have investigated and verified the feasibility of using electrode materials such as platinum, polyaniline, and boron-doped diamond to electrocatalyze the oxidation of phenol to p-benzoquinone. However, these electrocatalytic oxidation reactions reported in the literature are all carried out in non-aqueous media or strong acid conditions, and the conversion rate of phenol (<60%) and the yield of p-benzoquinone (<50%) are generally low. Therefore, in order to achieve the removal and resource utilization of phenol in wastewater, it is crucial to develop efficient, durable and easy-to-prepare electrode materials that can selectively convert phenol pollutants into p-benzoquinone at room temperature. Summary of the invention

[0005] In view of this, the purpose of the present invention is to propose a method for realizing the resource recovery of phenol pollutants in water by using nickel-ruthenium hybrid electrocatalysts, the characteristics of which are: designing and preparing a highly active nickel-ruthenium hybrid catalyst, which can simultaneously realize the removal of phenol pollutants in water and the selective generation of high-value para-benzoquinone.

[0006] The specific technical solution for achieving the purpose of the present invention is:

[0007] A method for realizing resource recovery of phenol pollutants in water by using a nickel-ruthenium hybrid catalyst comprises the following steps:

[0008] Step 1: dissolve nickel nitrate in pure water solution, stir evenly with magnetic force and set aside; wherein the concentration of nickel nitrate is 40.0-80.0 mmol / L;

[0009] Step 2: dissolving ruthenium trichloride in a dilute hydrochloric acid solution, stirring evenly with a magnetic force and setting aside; wherein the concentration of ruthenium trichloride is 0.5-2.0 mmol / L; the concentration of dilute hydrochloric acid is 0.1 mol / L;

[0010] Step 3: using the solution obtained in step 1 as an electrolyte, using carbon cloth as a cathode, and adopting a three-electrode system to prepare a nickel-carbon porous electrode by an electrodeposition method; wherein the negative potential applied by electrochemical deposition is 0.5-1.0 V; the deposition time is 5-15 min; a titanium sheet is used as a counter electrode, and a silver / silver chloride electrode is used as a reference electrode;

[0011] Step 4: using the solution obtained in step 2 as an electrolyte, using the nickel-carbon electrode obtained in step 3 as a substrate, and again using an electrochemical deposition method to prepare a nickel-ruthenium hybrid electrocatalyst supported on a carbon cloth; wherein the negative potential applied for electrochemical deposition is 0.2-0.6 V; the deposition time is 2-5 min; a titanium sheet is used as a counter electrode, and a silver / silver chloride electrode is used as a reference electrode;

[0012] Step 5: Dissolve phenol and sodium sulfate in ultrapure water, stir them evenly with a magnetic force, and mark them as the anolyte; dissolve an equal amount of sodium sulfate in ultrapure water, stir them evenly with a magnetic force, and mark them as the catholyte; wherein the concentration of phenol is 0.5-10.0 mmol / L; the concentration of sodium sulfate is 10-100 mmol / L; the initial pH of the anolyte and catholyte is 3.0-9.0, and the reagent for adjusting the pH value of the solution is 0.1 mol / L sulfuric acid or 0.1 mol / L sodium hydroxide solution;

[0013] Step 6: injecting the anolyte and catholyte prepared in step 5 into the anode chamber and cathode chamber of the H-type electrolytic cell respectively; using the nickel ruthenium carbon porous electrode prepared in step 4 as the anode, and using a three-electrode system to perform an electrocatalytic oxidation reaction;

[0014] Step 7: Continuously introduce argon gas into the anode chamber and apply a constant current to start the phenol electrocatalytic oxidation reaction. After a period of reaction, the selective conversion of phenol pollutants into high-value p-benzoquinone chemicals can be achieved; wherein, the applied constant current is 1~3mA; and the reaction time is 150 min.

[0015] Compared with other prior arts, the present invention has the following advantages:

[0016] (1) The nickel-ruthenium hybrid catalyst used in the present invention has a simple preparation process, high stability, and high selectivity for the oxidation of phenol pollutants.

[0017] (2) When using the new electrocatalytic oxidation system constructed by the present invention to treat phenol pollutants in water, it can not only effectively avoid the limitations of traditional electrocatalytic oxidation methods such as high energy consumption, high material consumption and high carbon emissions, but also achieve effective recovery of high-value benzoquinone chemicals.

[0018] (3) The nickel-ruthenium hybrid catalyst prepared by the present invention can achieve a higher phenol conversion rate and p-benzoquinone yield, and has high anti-interference ability and can operate in a complex water environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a spherical aberration transmission electron microscopy image of the nickel-ruthenium-carbon electrode in Example 1;

[0020] Figure 2 This is a performance comparison diagram of phenol removal and p-benzoquinone yield under different electrode conditions in Examples 1 to 3;

[0021] Figure 3 This is a graph showing the cyclic performance of the nickel-ruthenium-carbon electrode in Example 1;

[0022] Figure 4It is a performance comparison diagram of phenol removal and p-benzoquinone yield of Example 1 and Comparative Examples 2-4 under different initial pH conditions;

[0023] Figure 5 This is a performance diagram of phenol removal and benzoquinone yield in actual wastewater in Example 4. DETAILED DESCRIPTION

[0024] In order to better understand the content of the present invention, the technical solution of the present invention is further described below through specific examples, comparative examples and drawings. However, these examples do not limit the protection scope of the present invention.

[0025] Example 1

[0026] (1) Dissolve 60 mmol / L nickel nitrate in 100 mL pure water solution, stir magnetically and set aside;

[0027] (2) Dissolve 1.5 mmol / L ruthenium trichloride in 100 mL 0.1 mol / L dilute hydrochloric acid solution, stir magnetically and set aside;

[0028] (3) The solution obtained in step 1 is used as an electrolyte, a carbon cloth is used as a cathode, and a nickel-carbon porous electrode is prepared by an electrodeposition method using a three-electrode system; wherein the negative potential applied for electrochemical deposition is 1.0 V; the deposition time is 10 min; a titanium sheet is used as a counter electrode, and a silver / silver chloride electrode is used as a reference electrode;

[0029] (4) Using the solution obtained in step 2 as an electrolyte and the nickel-carbon electrode obtained in step 3 as a substrate, an electrochemical deposition method is again used to prepare a nickel-ruthenium hybrid electrocatalyst supported on a carbon cloth; wherein the negative potential applied in the electrochemical deposition is 0.5 V; the deposition time is 3 min; a titanium sheet is used as a counter electrode, and a silver / silver chloride electrode is used as a reference electrode;

[0030] (5) Dissolve 0.5 mmol / L phenol and 100 mmol / L sodium sulfate in 50 mL ultrapure water, stir magnetically to make it uniform, and mark it as the anolyte; dissolve an equal amount of sodium sulfate in ultrapure water, stir magnetically to make it uniform, and mark it as the catholyte; the initial pH of the anolyte and catholyte is 7.0, and the reagent for adjusting the pH value of the solution is 0.1 mol / L sulfuric acid solution;

[0031] (6) injecting the anolyte and catholyte prepared in step 5 into the anode chamber and cathode chamber of the H-type electrolytic cell respectively; using the nickel ruthenium carbon porous electrode prepared in step 4 as the anode, and using a three-electrode system to carry out an electrocatalytic oxidation reaction;

[0032] (7) Argon gas was continuously introduced into the anode chamber and a constant current of 2 mA was applied to initiate the electrocatalytic oxidation reaction of phenol. After 150 min of reaction, the selective conversion efficiency of phenol pollutants into high-value p-benzoquinone chemicals was evaluated.

[0033] The spherical aberration transmission electron microscopy image of the nickel ruthenium carbon porous electrode prepared in Example 1 is as follows Figure 1 As shown. Figure 2 The results show that, using the nickel-ruthenium-carbon porous electrode, 96.5% of phenol in water can be removed within 150 minutes, and the yield of p-benzoquinone can reach 83.4%. This result shows that the electrocatalytic oxidation system with nickel-ruthenium-carbon as the anode can simultaneously achieve the removal of phenol and the selective generation of high-value-added p-benzoquinone under ambient conditions. In addition, after the nickel-ruthenium-carbon electrode was recycled for 5 times, its catalytic activity was not significantly inhibited, indicating that it has high stability ( Figure 3 ).

[0034] Example 2

[0035] (1) Dissolve 60 mmol / L nickel nitrate in 100 mL pure water solution, stir magnetically and set aside;

[0036] (2) using the solution obtained in step 1 as an electrolyte, using carbon cloth as a cathode, and adopting a three-electrode system to prepare a nickel-carbon porous electrode by an electrodeposition method; wherein the negative potential applied for electrochemical deposition is 1.0 V; the deposition time is 10 min; a titanium sheet is used as a counter electrode, and a silver / silver chloride electrode is used as a reference electrode;

[0037] (3) Dissolve 0.5 mmol / L phenol and 100 mmol / L sodium sulfate in 50 mL ultrapure water, stir magnetically to make it uniform, and mark it as the anolyte; dissolve an equal amount of sodium sulfate in ultrapure water, stir magnetically to make it uniform, and mark it as the catholyte; the initial pH of the anolyte and catholyte is 7.0, and the reagent for adjusting the pH value of the solution is 0.1 mol / L sulfuric acid solution;

[0038] (4) injecting the anolyte and catholyte prepared in step 3 into the anode chamber and cathode chamber of the H-type electrolytic cell respectively; using the nickel-carbon porous electrode prepared in step 2 as the anode, and using a three-electrode system to carry out an electrocatalytic oxidation reaction;

[0039] (5) Argon gas was continuously introduced into the anode chamber and a constant current of 2 mA was applied to initiate the electrocatalytic oxidation reaction of phenol. After 150 min of reaction, the selective conversion efficiency of phenol pollutants into high-value p-benzoquinone chemicals was evaluated.

[0040] Depend on Figure 2It was found that when the nickel-carbon electrode was used as the anode, 73.7% of phenol in water could be removed within 150 min, but the yield of p-benzoquinone was only 16.1%, indicating that the nickel catalyst had no selectivity for the catalytic oxidation of phenol to p-benzoquinone.

[0041] Example 3

[0042] (1) Dissolve 1.5 mmol / L ruthenium trichloride in 100 mL 0.1 mol / L dilute hydrochloric acid solution, stir magnetically and set aside;

[0043] (2) The solution obtained in step 1 is used as an electrolyte, a carbon cloth is used as a cathode, and a nickel-carbon porous electrode is prepared by an electrodeposition method using a three-electrode system; wherein the negative potential applied for electrochemical deposition is 0.5 V; the deposition time is 3 min; a titanium sheet is used as a counter electrode, and a silver / silver chloride electrode is used as a reference electrode;

[0044] (3) Dissolve 0.5 mmol / L phenol and 100 mmol / L sodium sulfate in 50 mL ultrapure water, stir magnetically to make it uniform, and mark it as the anolyte; dissolve an equal amount of sodium sulfate in ultrapure water, stir magnetically to make it uniform, and mark it as the catholyte; the initial pH of the anolyte and catholyte is 7.0, and the reagent for adjusting the pH value of the solution is 0.1 mol / L sodium hydroxide solution;

[0045] (4) injecting the anolyte and catholyte prepared in step 3 into the anode chamber and cathode chamber of the H-type electrolytic cell respectively; using the ruthenium carbon porous electrode prepared in step 2 as the anode, and using a three-electrode system to carry out an electrocatalytic oxidation reaction;

[0046] (5) Argon gas was continuously introduced into the anode chamber and a constant current of 2 mA was applied to initiate the electrocatalytic oxidation reaction of phenol. After 150 min of reaction, the selective conversion efficiency of phenol pollutants into high-value p-benzoquinone chemicals was evaluated.

[0047] Depend on Figure 2 It can be seen that when the ruthenium carbon electrode is used as the anode, 59.3% of phenol in water can be removed within 150 minutes, but the yield of p-benzoquinone is 43.7%, and its p-benzoquinone selectivity can reach 73.7%, indicating that the ruthenium catalyst has selectivity for the catalytic oxidation of phenol to p-benzoquinone, but its phenol conversion rate and p-benzoquinone yield are still low. Compared with the catalytic performance of the nickel-ruthenium carbon electrode, it can be found that the introduction of nickel can promote the directional conversion of phenol to p-benzoquinone by the ruthenium carbon electrode.

[0048] Comparative Example 1

[0049] The difference between this comparative example and Example 1 is that the initial pH of the two electrolytes in step (5) is adjusted to 3.0 using 0.1 mol / L hydrochloric acid solution.

[0050] Comparative Example 2

[0051] The difference between this comparative example and Example 1 is that the initial pH of the two electrolytes in step (5) is adjusted to 5.0 using 0.1 mol / L hydrochloric acid solution.

[0052] Comparative Example 3

[0053] The difference between this comparative example and Example 1 is that the initial pH of the two electrolytes in step (5) is adjusted to 9.0 using 0.1 mol / L sodium hydroxide solution.

[0054] The removal of phenol and the yield of p-benzoquinone by the electrocatalytic oxidation system under different initial pH conditions in Example 1 and Comparative Examples 1 to 3 are as follows: Figure 5 The results show that the nickel-ruthenium-carbon electrode can achieve the directional conversion of phenol to p-benzoquinone in a wide pH range.

[0055] Example 4

[0056] (1) Dissolve 60 mmol / L nickel nitrate in 100 mL pure water solution, stir magnetically and set aside;

[0057] (2) Dissolve 1.5 mmol / L ruthenium trichloride in 100 mL 0.1 mol / L dilute hydrochloric acid solution, stir magnetically and set aside;

[0058] (3) The solution obtained in step 1 is used as an electrolyte, a carbon cloth is used as a cathode, and a nickel-carbon porous electrode is prepared by an electrodeposition method using a three-electrode system; wherein the negative potential applied for electrochemical deposition is 1.0 V; the deposition time is 10 min; a titanium sheet is used as a counter electrode, and a silver / silver chloride electrode is used as a reference electrode;

[0059] (4) Using the solution obtained in step 2 as an electrolyte and the nickel-carbon electrode obtained in step 3 as a substrate, an electrochemical deposition method is again used to prepare a nickel-ruthenium hybrid electrocatalyst supported on a carbon cloth; wherein the negative potential applied in the electrochemical deposition is 0.5 V; the deposition time is 3 min; a titanium sheet is used as a counter electrode, and a silver / silver chloride electrode is used as a reference electrode;

[0060] (5) 50 mL of actual coking wastewater containing 10.0 mmol / L phenol was marked as the anolyte; 100 mmol / L sodium sulfate was dissolved in 50 mL of ultrapure water, and after magnetic stirring, it was marked as the catholyte; the initial pH of the anolyte and catholyte was 7.0, and the reagent for adjusting the pH value of the solution was 0.1 mol / L sodium hydroxide solution;

[0061] (6) injecting the anolyte and catholyte prepared in step 5 into the anode chamber and cathode chamber of the H-type electrolytic cell respectively; using the nickel ruthenium carbon porous electrode prepared in step 4 as the anode, and using a three-electrode system to carry out an electrocatalytic oxidation reaction;

[0062] (7) Argon gas was continuously introduced into the anode chamber and a constant current of 2 mA was applied to initiate the electrocatalytic oxidation reaction of phenol. After 150 min of reaction, the selective conversion efficiency of phenol pollutants into high-value p-benzoquinone chemicals was evaluated.

[0063] Example 4 The electrocatalytic oxidation efficiency of phenol in actual coking wastewater is as follows Figure 5 The results show that the electrocatalytic oxidation system with nickel ruthenium carbon as the anode can achieve 68.1% removal of phenol within 24 hours, and the yield of benzoquinone can reach 52.3%. This performance shows that the electrocatalyst of the present invention has good application prospects in the resource utilization of phenol-containing wastewater.

[0064] It can be seen from the above embodiments that the present invention provides a method for selectively converting phenol in water to p-benzoquinone by electrocatalytic oxidation. The method of the present invention can not only achieve the effect of purifying wastewater, but also simultaneously realize the recovery of high value-added organic resources.

[0065] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for realizing resource recovery of phenol pollutants in water using nickel-ruthenium hybrid electrocatalysts. It is characterized in that The following steps are involved: Step 1: dissolve nickel nitrate in pure water solution, stir evenly with magnetic force and set aside; wherein the concentration of nickel nitrate is 40.0-80.0 mmol / L; Step 2: dissolving ruthenium trichloride in a dilute hydrochloric acid solution, stirring evenly with a magnetic force and setting aside; wherein the concentration of ruthenium trichloride is 0.5-2.0 mmol / L; the concentration of dilute hydrochloric acid is 0.1 mol / L; Step 3: using the solution obtained in step 1 as an electrolyte, using carbon cloth as a cathode, and using a three-electrode system to prepare a nickel-carbon porous electrode by an electrodeposition method; wherein the negative potential applied by electrochemical deposition is 0.5-1.0 V; the deposition time is 5-15 min; a titanium sheet is used as a counter electrode, and a silver / silver chloride electrode is used as a reference electrode; Step 4: using the solution obtained in step 2 as an electrolyte, using the nickel-carbon electrode obtained in step 3 as a substrate, and again using an electrochemical deposition method to prepare a nickel-ruthenium hybrid electrocatalyst supported on a carbon cloth; wherein the negative potential applied for electrochemical deposition is 0.2-0.6 V; the deposition time is 2-5 min; a titanium sheet is used as a counter electrode, and a silver / silver chloride electrode is used as a reference electrode; Step 5: Dissolve phenol and sodium sulfate in ultrapure water, stir them evenly with a magnetic force, and mark them as the anolyte; dissolve an equal amount of sodium sulfate in ultrapure water, stir them evenly with a magnetic force, and mark them as the catholyte; wherein the concentration of phenol is 0.5-10.0 mmol / L; the concentration of sodium sulfate is 10-100 mmol / L; the initial pH of the anolyte and catholyte is 3.0-9.0, and the reagent for adjusting the pH value of the solution is 0.1 mol / L sulfuric acid or 0.1 mol / L sodium hydroxide solution; Step 6: injecting the anolyte and catholyte prepared in step 5 into the anode chamber and cathode chamber of the H-type electrolytic cell respectively; using the nickel ruthenium carbon porous electrode prepared in step 4 as the anode, and using a three-electrode system to perform an electrocatalytic oxidation reaction; Step 7: Continuously introduce argon gas into the anode chamber and apply a constant current to start the phenol electrocatalytic oxidation reaction. After a period of reaction, the selective conversion of phenol pollutants into high-value p-benzoquinone chemicals can be achieved; wherein, the applied constant current is 1~3 mA; and the reaction time is 150 min.

Citation Information

Patent Citations

  • Method for preparing cyclohexane by catalyzing and hydrogenising benzene at room temperature

    CN102746087A

  • Metal ruthenium-based electrode and preparation method and application thereof

    CN113603191A

  • Method for selectively converting phenol in water into p-benzoquinone by utilizing electrocatalytic oxidation method

    CN116375149A

  • Method for electrochemically catalyzing phenol-containing wastewater into high-added-value chemicals

    CN118164591A