Iron ion slow-release hydrogel ball as well as preparation method and application thereof

By preparing iron ion slow-release hydrogel spheres, the problems of high Fe2+ consumption, excessive iron sludge generation, and narrow pH range in Fenton technology were solved, achieving a highly efficient wastewater treatment effect and avoiding secondary pollution from the loss of metal sulfides.

CN118929885AInactive Publication Date: 2024-11-12INNOVATION CENTER OF YANGTZE RIVER DELTA ZHEJIANG UNIVERSITY

Patent Information

Application Number
CN202410943243.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Fenton technology has several drawbacks in wastewater treatment, including a narrow applicable pH range, low H2O2 utilization efficiency, high Fe2+ consumption, slow conversion of Fe3+ to Fe2+, and large amount of iron sludge formation. Furthermore, the loss of metal sulfides causes secondary pollution.

Method used

Iron ion slow-release hydrogel spheres were prepared by crosslinking a sodium alginate/polyvinylpyrrolidone solution containing CoS2 powder with a ferrous ion solution, thus constructing a CoS2/Fe/SA/H2O2 heterogeneous Fenton system. CoS2 was used to promote the conversion of Fe3+ to Fe2+, reduce the generation of iron sludge, expand the applicable pH range, and improve the utilization rate of Fe2+.

Benefits of technology

It achieves continuous and stable release of Fe2+, avoids rapid consumption and iron sludge formation, expands the applicable pH range, improves the degradation efficiency of new pollutants, and reduces secondary pollution from the loss of metal sulfides, thus having broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929885A_ABST
    Figure CN118929885A_ABST
Patent Text Reader

Abstract

The invention discloses an iron ion slow-release hydrogel ball and a preparation method and application thereof. The preparation method comprises the following steps: adding CoS2 powder into an aqueous solution containing sodium alginate and polyvinylpyrrolidone, stirring to obtain a mixed solution A, dropwise adding the mixed solution A into a ferrite solution, and stirring to carry out a cross-linking reaction. According to the invention, a sodium alginate / polyvinylpyrrolidone solution dispersed with CoS2 powder and a ferrous ion solution are subjected to a cross-linking reaction; the prepared iron ion slow-release hydrogel ball can continuously and stably release Fe < 2 + >, avoids rapid consumption of Fe < 2 + > and generation of iron mud, is wide in pH application range, and has excellent degradation performance on new pollutants in a water body. When the hydrogel ball is used for degrading new pollutants in a water body, the concentration of Fe < 2 + > in a system is basically kept stable; and the hydrogel balls keep a complete form in water, so that solid-liquid separation and recovery of a cocatalyst CoS2 are facilitated, and secondary pollution caused by loss of metal sulfides is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of sewage treatment, and specifically relates to an iron ion slow-release hydrogel ball and a preparation method and application thereof. Background Art

[0002] Advanced oxidation processes (AOPs) with hydroxyl radicals (·OH) as the main active substance are considered to be one of the effective methods for degrading new pollutants. Among them, Fenton technology is one of the most widely used AOPs due to its high efficiency and simple operation. It plays a pivotal role in sewage treatment, landfill leachate treatment, water environment remediation and other fields. However, Fenton technology has the disadvantages of narrow pH range (usually 3-4), low H2O2 utilization efficiency, and Fe 2+ Fast consumption, Fe 3+ Fe 2+ Problems such as slow conversion and large amount of iron sludge generated limit its wider application.

[0003] In order to solve the above problems, people have tried to introduce reducing substances as co-catalysts in the Fenton system. Studies have found that transition metal sulfides represented by MoS2 and CoS2 can simultaneously use S and transition metals to reduce Fe 3+ , thereby accelerating Fe 3+ / Fe 2+ conversion, reducing iron sludge generation, greatly improving reaction efficiency, and is considered to be an excellent co-catalyst. However, adding metal sulfide and Fe 2+ , which will cause Fe 2+ There are problems such as large consumption and failure to effectively utilize, and the loss of metal sulfides causing secondary pollution.

[0004] The patent document with publication number CN111732181A discloses a multiphase Fenton reagent and its application. The multiphase Fenton reagent provided by the invention includes ferrous disulfide, hydrogen peroxide and transition metal sulfide; the transition metal sulfide includes one or more of molybdenum disulfide, zinc sulfide and tungsten disulfide; the hydrogen peroxide is independently packaged. In the multiphase Fenton reagent provided by the invention, the transition metal sulfide acts as a co-catalyst, which can timely reduce trivalent ferrous ions to ferrous ions and continue to decompose hydrogen peroxide to produce hydroxyl radicals to degrade pollutants. Moreover, the transition metal sulfide acts as a co-catalyst, and its own performance will not be damaged. It can continuously and stably play a co-catalyst role, thereby improving the generation efficiency and stability of divalent ferrous ions on the surface of ferrous disulfide. However, the Fe 2+ The large consumption and loss of metal sulfide will cause secondary pollution to the environment.

[0005] As a hydrophilic three-dimensional network structure material, hydrogel is widely used in the fields of medicine and water treatment due to its drug release and excellent adsorption properties. Among them, sodium alginate (SA) is a natural polysaccharide extracted from plants such as seaweed and kelp. It has good stability, is non-toxic and easily biodegradable. It can cross-link with multivalent cations to form a solid hydrogel; at the same time, sodium alginate can load nano-scale particles to form a composite hydrogel.

[0006] Therefore, in view of the above-mentioned deficiencies in the prior art, a hydrogel ball with a slow-release effect of iron ions is prepared and used to activate hydrogen peroxide to form a Fenton-like reaction, thereby solving the problems of the narrow pH application range of the traditional Fenton reaction, low H2O2 utilization efficiency, and Fe 2+ High consumption, Fe 3+ Fe 2+ Problems such as slow conversion and large amount of iron sludge generation are of great significance. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides an iron ion sustained-release hydrogel ball and its preparation method and application. The present invention adopts sodium alginate (SA) / polyvinyl pyrrolidone (PVP) solution dispersed with CoS2 powder and ferrous ion solution to cross-link and prepare hydrogel balls (CoS2 / Fe / SA hydrogel balls) with iron ion sustained-release effect. 2+ The heterogeneous Fenton system of CoS2 / Fe / SA / H2O2 was constructed to improve the Fe 2+ utilization rate, expanded the pH application range, and promoted Fe 3+ Fe 2+ The conversion reduces the generation of iron sludge and ultimately improves the degradation efficiency of new pollutants in the water.

[0008] The first aspect of the present invention provides a method for preparing an iron ion sustained-release hydrogel sphere, comprising the following steps:

[0009] CoS2 powder is added to an aqueous solution containing sodium alginate and polyvinyl pyrrolidone, and stirred to obtain a mixed solution A. The mixed solution A is dropped into a ferrous salt solution and stirred to perform a cross-linking reaction to obtain the iron ion sustained-release hydrogel sphere, i.e., CoS2 / Fe / SA hydrogel sphere.

[0010] Sodium alginate has good biocompatibility and degradability. As the matrix material of hydrogel, the molecular chain of sodium alginate contains a large number of carboxyl groups, which can react with Fe 2+Chelation occurs to form a network structure, providing the hydrogel with a basic shape and mechanical strength, which can stably release iron ions. Polyvinyl pyrrolidone is used as a thickener to help adjust the viscosity and stability of the sodium alginate solution, promote the formation of the hydrogel, improve the structural stability, and facilitate recycling. During the cross-linking process, Fe 2+ The ions are evenly dispersed in the sodium alginate / polyvinyl pyrrolidone network to form hydrogel spheres with sustained release of iron ions. 2+ It is a key catalyst in the Fenton reaction, which can catalyze the decomposition of hydrogen peroxide (H2O2) to generate hydroxyl radicals (·OH), thereby achieving the degradation of new pollutants. CoS2, as a co-catalyst, can promote the degradation of Fe 3+ Fe 2+ The reduction of Fe 2+ concentration, increasing Fe 2+ The utilization rate of CoS2 is improved, the generation of iron sludge is reduced, and the applicable pH range of the reaction is broadened; at the same time, the catalytic effect of CoS2 combined with the sustained release effect of SA / PVP hydrogel can further improve the efficiency of the Fenton reaction.

[0011] The present invention uses the synergistic effect of the above substances to finally prepare a product that can continuously and stably release Fe 2 + , avoiding Fe 2+ Iron ion slow-release hydrogel spheres with rapid consumption and iron sludge production, wide pH range of application and high degradation rate for new pollutants.

[0012] Preferably, the mass ratio of sodium alginate to polyvinyl pyrrolidone is 2.5-7.5:1.

[0013] Preferably, in the aqueous solution, the concentration of sodium alginate is 0.01-0.03 g / mL, and the concentration of polyvinyl pyrrolidone is 0.002-0.01 g / mL.

[0014] Preferably, the mass ratio of the CoS2 powder to sodium alginate is 0.05 to 0.35: 1. Further preferably, the mass ratio of the CoS2 powder to sodium alginate is 0.05 to 0.25: 1. More preferably, the mass ratio of the CoS2 powder to sodium alginate is 0.15: 1. This ratio of CoS2 powder to sodium alginate can ensure the formation of hydrogel balls with a stable structure and ensure that it has a good catalytic effect.

[0015] Preferably, the ferrous salt includes FeSO4 or FeCl2, and the mass ratio of the ferrous salt to sodium alginate is 2 to 8:1.

[0016] Preferably, the mass fraction of the ferrous salt solution is 2-20 wt%. 2+ The concentration is controlled to adjust the number of cycles of the hydrogel spheres to meet the needs of practical applications.

[0017] Preferably, the ferrous salt is FeCl2, the mass ratio of FeCl2 to sodium alginate is 2-3:1, and the mass fraction of the FeCl2 solution is 2-4wt%. Under this condition, FeCl2 and SA can be cross-linked to form CoS2 / Fe / SA hydrogel spheres with good physical and chemical properties, and sufficient Fe can be slowly released when constructing a heterogeneous Fenton system. 2+ ions, ensuring that the model pollutants are completely degraded.

[0018] Preferably, the cross-linking reaction time is 8 to 15 hours. Under this condition, SA and Fe 2+ The hydrogel balls formed by full contact and cross-linking have a stable structure without gaps and cracks.

[0019] Preferably, the cross-linking reaction is carried out in a hypoxic or anaerobic environment. The cross-linking reaction is carried out under hypoxic or anaerobic conditions to prevent Fe 2+ Oxidized to Fe 3+ , ensuring that the hydrogel balls release Fe 2+ performance.

[0020] The present invention also provides an iron ion sustained-release hydrogel ball prepared by the above-mentioned preparation method. The iron ion sustained-release hydrogel ball is Fe 2+ Ions can be continuously and stably released from CoS2 / Fe / SA hydrogel spheres, and Fe 2+ The concentration can be stabilized without the need to add additional Fe 2+ ions, and has a wide pH range of application.

[0021] The present invention also provides the use of the iron ion slow-release hydrogel ball in degrading new pollutants in water. 2+ Constructing a CoS2 / Fe / SA / H2O2 heterogeneous Fenton system and activating hydrogen peroxide to form a Fenton-like reaction can significantly increase the Fe 2+ utilization rate, expand the pH range, and promote Fe 3+ Fe 2+ It can reduce the generation of iron sludge and has a very high degradation efficiency for new pollutants in water bodies, and has broad application prospects in the field of sewage treatment.

[0022] Compared with the prior art, the present invention has at least the following beneficial effects:

[0023] (1) The present invention uses a sodium alginate / polyvinyl pyrrolidone solution dispersed with CoS2 powder and a ferrous ion solution to carry out a cross-linking reaction, and finally prepares a ferrous ion solution that can continuously and stably release Fe through the synergistic effect of the above substances. 2+ , avoiding Fe 2+ Iron ion slow-release hydrogel spheres with rapid consumption and iron sludge production, wide pH range of application, and excellent degradation performance for new pollutants in water bodies.

[0024] (2) The iron ion slow-release hydrogel spheres (CoS2 / Fe / SA hydrogel spheres) prepared by the present invention are used to construct the CoS2 / Fe / SA / H2O2 heterogeneous Fenton system for the degradation of new pollutants in water. During the degradation process, Fe 2+ It is slowly released from the CoS2 / Fe / SA hydrogel spheres. After a certain period of time, the Fe 2+ The concentration remains basically stable, and no additional Fe addition is required 2+ ; Moreover, the CoS2 / Fe / SA hydrogel balls can maintain their complete shape in water before and after the reaction, which is beneficial to solid-liquid separation and the recovery of the co-catalyst CoS2, avoiding the loss of metal sulfide to form secondary pollution.

[0025] (3) The present invention uses sodium alginate as the main raw material, which has low cost, small dosage, simple preparation process, no biological toxicity and can be biodegraded, and the prepared hydrogel spheres can be recycled; and the present invention can adjust the cross-linking time Fe 2+ The concentration of the hydrogel spheres can be used to control the number of cycles to meet the needs of practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The removal effects of model pollutants by traditional Fenton system, heterogeneous system and CoS2 / Fe / SA / H2O2 heterogeneous Fenton system.

[0027] Figure 2 This is the degradation effect of the CoS2 / Fe / SA / H2O2 heterogeneous Fenton system at different pH values.

[0028] Figure 3 The release of Fe from CoS2 / Fe / SA hydrogel spheres during the reaction 2+ situation.

[0029] Figure 4 The recycling performance of CoS2 / Fe / SA hydrogel prepared in Examples 1, 6 to 8, wherein Figure 4 a is the hydrogel prepared in Example 1; Figure 4 b is the hydrogel prepared in Example 6; Figure 4 c is the hydrogel prepared in Example 7; Figure 4d is the hydrogel prepared in Example 8. DETAILED DESCRIPTION

[0030] In order to deepen the understanding of the present invention, the embodiments of the present invention are described in detail below in conjunction with the drawings and embodiments.

[0031] Unless otherwise specified, the equipment used in this example is conventional experimental equipment, and the materials and reagents used are commercially available unless otherwise specified.

[0032] Example 1

[0033] (1) Weigh 1 g SA (sodium alginate, S100128, Aladdin) and 0.2 g PVP into 50 ml ultrapure water, and add 0.15 g CoS2 powder into the water and stir for 6 h to dissolve SA and PVP and evenly disperse CoS2 to form a mixed solution A.

[0034] (2) Dissolve 4 g of FeCl2·4H2O in 96 ml of ultrapure water and stir for 15 min to form solution B.

[0035] (3) The mixed solution A was drawn up with a syringe and dripped into the solution B drop by drop, and the mixture was stirred for 12 h for cross-linking reaction. During the cross-linking process, the mouth of the beaker was covered with a sealing film to obtain CoS2 / Fe / SA hydrogel spheres.

[0036] (4) The CoS2 / Fe / SA hydrogel spheres were taken out and washed with ultrapure water to finally obtain spherical CoS2 / Fe / SA hydrogel.

[0037] Example 2

[0038] (1) Weigh 0.5 g SA (sodium alginate, S100128, Aladdin) and 0.2 g PVP in 50 ml ultrapure water, add 0.15 g CoS2 powder and stir for 6 h to dissolve SA and PVP and evenly disperse CoS2 to form a mixed solution A.

[0039] (2) Dissolve 4 g of FeCl2·4H2O in 96 ml of ultrapure water and stir for 15 min to form solution B.

[0040] (3) The mixed solution A was drawn up with a syringe and dripped into the solution B drop by drop, and the mixture was stirred for 12 h for cross-linking reaction. During the cross-linking process, the mouth of the beaker was covered with a sealing film to obtain CoS2 / Fe / SA hydrogel spheres.

[0041] (4) The CoS2 / Fe / SA hydrogel spheres were taken out and washed with ultrapure water to finally obtain spherical CoS2 / Fe / SA hydrogel.

[0042] Example 3

[0043] (1) Weigh 1.5 g SA (sodium alginate, S100128, Aladdin) and 0.2 g PVP in 50 ml ultrapure water, add 0.15 g CoS2 powder and stir for 6 h to dissolve SA and PVP and evenly disperse CoS2 to form a mixed solution A.

[0044] (2) Dissolve 4 g of FeCl2·4H2O in 96 ml of ultrapure water and stir for 15 min to form solution B.

[0045] (3) The mixed solution A was drawn up with a syringe and dripped into the solution B drop by drop, and the mixture was stirred for 12 h for cross-linking reaction. During the cross-linking process, the mouth of the beaker was covered with a sealing film to obtain CoS2 / Fe / SA hydrogel spheres.

[0046] (4) The CoS2 / Fe / SA hydrogel spheres were taken out and washed with ultrapure water to finally obtain spherical CoS2 / Fe / SA hydrogel.

[0047] Example 4

[0048] (1) Weigh 1.0 g of SA (sodium alginate, S100128, Aladdin) and 0.2 g of PVP in 50 ml of ultrapure water, and add 0.05 g of CoS2 powder into each of them and stir for 6 h to dissolve SA and PVP and evenly disperse CoS2 to form a mixed solution A.

[0049] (2) Dissolve 4 g of FeCl2·4H2O in 96 ml of ultrapure water and stir for 15 min to form solution B.

[0050] (3) The mixed solution A was drawn up with a syringe and dripped into the solution B drop by drop, and the mixture was stirred for 12 h for cross-linking reaction. During the cross-linking process, the mouth of the beaker was covered with a sealing film to obtain CoS2 / Fe / SA hydrogel spheres.

[0051] (4) The CoS2 / Fe / SA hydrogel spheres were taken out and washed with ultrapure water to finally obtain spherical CoS2 / Fe / SA hydrogel.

[0052] Example 5

[0053] (1) Weigh 1.0 g of SA (sodium alginate, S100128, Aladdin) and 0.2 g of PVP in 50 ml of ultrapure water, and add 0.25 g of CoS2 powder into the water and stir for 6 h to dissolve SA and PVP and evenly disperse CoS2 to form a mixed solution A.

[0054] (2) Dissolve 4 g of FeCl2·4H2O in 96 ml of ultrapure water and stir for 15 min to form solution B.

[0055] (3) The mixed solution A was drawn up with a syringe and dripped into the solution B drop by drop, and the mixture was stirred for 12 h for cross-linking reaction. During the cross-linking process, the mouth of the beaker was covered with a sealing film to obtain CoS2 / Fe / SA hydrogel spheres.

[0056] (4) The CoS2 / Fe / SA hydrogel spheres were taken out and washed with ultrapure water to finally obtain spherical CoS2 / Fe / SA hydrogel.

[0057] Embodiments 6 to 8

[0058] Examples 6 to 8 respectively used 7.7wt%, 12.8wt%, and 17.9wt% FeCl2 solutions (prepared by dissolving FeCl2·4H2O in ultrapure water and stirring for 15 minutes) to prepare CoS2 / Fe / SA hydrogels, and the other conditions were the same as those in Example 1.

[0059] Comparative Example 1

[0060] (1) Weigh 1.0 g of SA (sodium alginate, S100128, Aladdin) and 0.2 g of PVP in 50 ml of ultrapure water without adding CoS2 powder and stir for 6 h to dissolve SA and PVP to form a mixed solution A.

[0061] (2) Dissolve 4 g of FeCl2·4H2O in 96 ml of ultrapure water and stir for 15 min to form a 4 wt% FeCl2·4H2O solution B.

[0062] (3) The mixed solution A was drawn up with a syringe and dripped into the solution B drop by drop, and the mixture was stirred for 12 h for cross-linking reaction. During the cross-linking process, the mouth of the beaker was covered with a sealing film to obtain CoS2 / Fe / SA hydrogel spheres.

[0063] (4) The CoS2 / Fe / SA hydrogel spheres were taken out and washed with ultrapure water to finally obtain spherical CoS2 / Fe / SA hydrogel.

[0064] Application Example 1

[0065] A 20 μmol / L carbamazepine (CBZ) solution was prepared and three parallel experiments were conducted, namely the Fe / H2O2 system, the Fe / CoS2 / H2O2 system and the CoS2 / Fe / SA / H2O2 system. The construction methods of the above three systems are:

[0066] Fe / H2O2 system: Prepare 200 ml of a model pollutant solution with a carbamazepine concentration of 20 μM and H2O2 of 4 mg / L, and add 2 mg of solid FeCl2·4H2O. 2+ The initial concentration was 2.8 mg / L.

[0067] Fe / CoS2 / H2O2 system: prepare 200 ml of model pollutant solution with carbamazepine concentration of 20 μM and H2O2 of 4 mg / L, add 2 mg of solid FeCl2·4H2O and 1 mg of CoS2 powder. 2+ The initial concentration was 2.8 mg / L and the CoS2 concentration was 5 mg / L.

[0068] CoS2 / Fe / SA / H2O2 system: Prepare 200 ml of a model pollutant solution with a carbamazepine concentration of 20 μM and H2O2 of 4 mg / L, and add 0.4 g of CoS2 / Fe / SA hydrogel spheres (Example 1). The dosage of CoS2 / Fe / SA hydrogel spheres in this system is 2 g / L. The Fe released by the hydrogel spheres in this system 2+ The concentration (maximum value) and the amount of CoS2 contained in the above system are 2+ The initial concentration and the amount of CoS2 added were equivalent.

[0069] like Figure 1 As shown in Figure 2, at 90 min, the degradation rate of carbamazepine by the CoS2 / Fe / SA / H2O2 system was 99.8%, and the reaction rate constant was 0.1846 min. -1 , and its degradation effect is better than that of Fe / H2O2 system and Fe / CoS2 / H2O2 system.

[0070] Application Example 2

[0071] A 20 μmol / L carbamazepine (CBZ) solution was prepared, and the CoS2 / Fe / SA hydrogel spheres prepared in Examples 4-5 were used to construct the CoS2 / Fe / SA / H2O2 system, and the construction method was the same as that in Application Example 1. At 90 min, the degradation rates of carbamazepine by the CoS2 / Fe / SA / H2O2 systems of Examples 4-5 were 99.4% and 99.6%, respectively.

[0072] The Fe / SA hydrogel prepared in Comparative Example 1 was used to construct the Fe / SA / H2O2 system. The construction method was as follows: 200 ml of a model pollutant solution with a carbamazepine concentration of 20 μM and H2O2 of 4 mg / L was prepared, and 0.4 g of Fe / SA hydrogel beads were added. The dosage of Fe / SA hydrogel beads in this system was 2 g / L. The degradation rate of carbamazepine by the hydrogel prepared in Comparative Example 1 was 98.3%, and the reaction rate constant was 0.1089 min -1 .

[0073] Application Example 3

[0074] A 20 μmol / L carbamazepine solution was prepared and the degradation experiment was carried out in an environment with a pH of 3 to 10. The Fe 2+Concentration changes. Figure 2 As shown, the CoS2 / Fe / SA / H2O2 system has good degradation effect at different pH values; Figure 3 It shows that Fe 2+ The ion concentration continued to increase and stabilized at around 1.56 mg / L.

[0075] Application Example 4

[0076] The CoS2 / Fe / SA hydrogel prepared in Example 1 and Examples 6 to 8 was used for the circulation experiment, and the dosage of carbamazepine and hydrogel spheres was 20 μmol / L and 2 g / L respectively. Figure 4 As shown, the number of cycles of the hydrogel spheres can be changed by adjusting the concentration of the FeCl2·4H2O solution during cross-linking.

Claims

1. A method for preparing iron ion sustained-release hydrogel spheres, characterized in that: The following steps are involved: CoS2 powder is added into an aqueous solution containing sodium alginate and polyvinyl pyrrolidone, and stirred to obtain a mixed solution A. The mixed solution A is dropped into a ferrous salt solution, and stirred to perform a cross-linking reaction to obtain the iron ion sustained-release hydrogel sphere.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the sodium alginate to polyvinyl pyrrolidone is 2.5-7.5:

1.

3. The preparation method according to claim 2, characterized in that: In the aqueous solution, the concentration of sodium alginate is 0.01-0.03 g / mL.

4. The preparation method according to claim 1, characterized in that: The mass ratio of the CoS2 powder to sodium alginate is 0.05-0.35:

1.

5. The preparation method according to claim 1, characterized in that: The ferrous salt includes FeSO4 or FeCl2, and the mass ratio of the ferrous salt to sodium alginate is 2 to 8:

1.

6. The preparation method according to claim 5, characterized in that: The mass fraction of the ferrous salt solution is 2-20wt%.

7. The preparation method according to claim 5 or 6, characterized in that: The ferrous salt is FeCl2, the mass ratio of FeCl2 to sodium alginate is 2-3:1, and the mass fraction of the FeCl2 solution is 2-4wt%.

8. The preparation method according to claim 1, characterized in that: The cross-linking reaction is carried out in a low-oxygen or anaerobic environment; the cross-linking reaction time is 8 to 15 hours.

9. The iron ion sustained-release hydrogel sphere prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the iron ion slow-release hydrogel sphere according to claim 9 in degrading new pollutants in water bodies.

Citation Information

Patent Citations

  • Sulfide-containing industrial wastewater treatment reagent and reaction method thereof

    CN107720930A

  • Polymer gel fenton catalyst, and preparation method and application thereof

    CN110548543A

  • Preparation method of 3D cobalt sulfide co-catalyst and application of co-catalysis Fenton reaction

    CN115106112A

  • Preparation method of sodium alginate hydrogel material for Fenton-like system to degrade organic pollutants in water body

    CN116273200A

Cited By

  • Method for degrading short-chain chlorinated paraffin in soil based on calcium sulfite-ferric sulfate double slow-release system

    CN121339175A