Preparation method and application of perovskite quantum dot double-spectrum luminescent glass material

By doping rare earth elements in perovskite quantum dots, the problems of insufficient stability and photoelectric performance of single halogen perovskites are solved, and the stable precipitation and broad-spectrum light emission of CsPbCl2Br1 quantum dots in glass are achieved, which improves the material's Environmental tolerance and photoelectric properties, suitable for a variety of photoelectric applications.

CN118930046APending Publication Date: 2024-11-12KUNMING UNIV OF SCI & TECH

Patent Information

Application Number
CN202411144127.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Single halogen perovskite quantum dots have shortcomings in environmental stability and photoelectric properties, which are difficult to meet the needs of different photoelectric applications, and there is a problem that CsPbCl2Br1 is difficult to precipitate during the preparation of mixed halogen perovskites.

Method used

High-temperature melting method is used to dopate rare earth elements into CsPbCl2Br1 quantum dots, making them easy to precipitate in glass substrates, and form stable perovskite quantum dots dual spectral luminescent glass materials, rare earth elements such as Nd2O3 or Er2O3 is used to improve the chemical stability and optical properties of materials.

Benefits of technology

The stable precipitation and broad-spectrum light emission of CsPbCl2Br1 quantum dots are realized, which improves the environmental tolerance and photoelectric performance of the material, enhances the application potential in display technology and optoelectronic devices, and achieves efficient luminescence in visible and near-infrared regions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930046A_ABST
    Figure CN118930046A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a perovskite quantum dot double-spectrum luminescent glass material, and belongs to the field of novel luminescent materials. The preparation method specifically comprises the following steps: firstly, fully mixing high-purity B2O3, SiO2, ZnO, Cs2CO3, SrO, PbBr2, PbCl2, NaBr, NaCl, Al2O3, SnO2 and a rare earth oxide, grinding, and calcining to obtain a glass melt; and pouring the glass melt into a preheated copper plate mold, and naturally cooling and molding to separate out CsPbCl2Br1 quantum dot glass, namely the perovskite quantum dot double-spectrum luminescent glass material. The stable CsPbCl2Br1 quantum dot glass material is successfully prepared by adding the rare earth oxide, the prepared CsPbCl2Br1 quantum dot glass material shows remarkable luminescence characteristics in visible light and near-infrared regions, the optical performance of perovskite quantum dots is further expanded, the perovskite quantum dots can efficiently emit light in the near-infrared band, and the application prospect is broad. And the requirements in the fields of optical communication, imaging, night vision equipment, safety detection and the like are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a perovskite quantum dot dual-spectrum luminescent glass material, belonging to the field of new luminescent materials. Background Art

[0002] In recent years, quantum dots (QDs) have attracted much attention in the fields of displays, photovoltaics, sensors, etc. due to their unique optoelectronic properties, such as wide absorption spectrum, narrow and tunable emission spectrum and high quantum yield. In particular, perovskite quantum dots (PQDs) have become a hot topic of research due to their simple synthesis, high luminous efficiency and pure color. However, perovskite quantum dots have poor stability in the environment and are easily affected by factors such as air, moisture, heat and light, resulting in a rapid decline in optoelectronic performance, which seriously limits their practical application.

[0003] Inorganic halide CsPbX3 (X = Cl, Br) perovskite quantum dots (Quantum dots, QDs) have excellent properties such as wide spectral tunable spectral range, high fluorescence quantum efficiency, narrow emission linewidth and easy synthesis, and show great potential in the fields of light-emitting diodes (Light-emittingdioeds, LEDs), lasers, solar cells, photodetectors and backlight displays. In particular, CsPbX3 QDs (X = Cl, Br) have been regarded as a substitute for traditional color converters in backlight displays, with excellent color gamut and reproducibility of liquid crystal displays (Liquid crystal display, LCD). Although CsPbX3 (X = Cl, Br) quantum dots are considered to be a hot material for backlight applications.

[0004] However, single halogen perovskite materials have the following problems:

[0005] (1) Single halogen perovskite materials generally have a narrow light absorption range. For example, CsPbCl3 mainly absorbs ultraviolet light, CsPbBr3 mainly absorbs blue light, and CsPbI3 absorbs red light. In contrast, mixed halogen perovskites can adjust the light absorption range by adjusting the halogen ratio to cover a wider spectral region, thereby improving the efficiency of optoelectronic devices.

[0006] (2) Difficulty in bandgap adjustment: Single-halogen perovskites have a fixed bandgap, which limits their applicability in different optoelectronic applications. Mixed-halogen perovskites can achieve continuous adjustment of the bandgap by adjusting the ratio of different halogens, giving them greater flexibility in different application requirements.

[0007] (3) Poor environmental stability: Single halogen perovskites generally have poor environmental stability. For example, CsPbI3 is easily degraded in humid environments, while CsPbCl3 and CsPbBr3 may show different stabilities under other environmental conditions. Mixed halogen perovskites can improve the environmental stability of materials and enhance their reliability in practical applications by combining different halogen elements.

[0008] (5) Electron mobility and photoelectric conversion efficiency: In some cases, the electron mobility and photoelectric conversion efficiency of single halogen perovskites may be lower than those of mixed halogen perovskites. Mixed halogen perovskites can optimize these performance parameters by adjusting the ratio of different halogens, thereby improving the overall performance of the device.

[0009] There are many problems with perovskites based on a single halogen, so researchers began to study mixed halogen perovskites. However, in the preparation process of mixed halogen perovskites, there is still the problem that CsPbCl2Br1 is difficult to precipitate.

[0010] The present invention aims at the problems existing in the existing perovskite quantum glass. The CsPbCl2Br1 quantum dots are easily precipitated in the glass matrix by doping with rare earth elements using a high-temperature melting method. The rare earth elements have good chemical stability and can improve the environmental tolerance of the perovskite material. They can form a stable composite material with the perovskite matrix and reduce the degradation of the perovskite under moisture or light.

[0011] Rare earth doping can reduce photodegradation and improve the performance stability of perovskite under long-term illumination. Summary of the invention

[0012] In order to solve the problems existing in the existing inorganic halide CsPbX3 (X = Cl, Br) perovskite quantum dots and the problems existing in the preparation process of polyhalogen perovskites, one of the purposes of the present invention is to provide a method for preparing a perovskite quantum dot dual-spectrum luminescent glass material, and the preparation method specifically comprises the following steps:

[0013] (1) High-purity B2O3, SiO2, ZnO, Cs2CO3, SrO, PbBr2, PbCl2, NaBr, NaCl, Al2O3, SnO2 and rare earth oxides are fully mixed and ground, and then calcined to obtain a glass melt, wherein the rare earth oxide is one of Nd2O3 and Er2O3.

[0014] (2) Pour the glass melt obtained in step (1) into a preheated copper plate mold, cool it naturally and form it, so as to obtain CsPbCl2Br1NCs perovskite quantum dot glass, which is a perovskite quantum dot dual-spectrum luminescent glass material.

[0015] Preferably, the molar percentage of the rare earth element added in step (1) is 1%-10% of the total amount of B2O3, SiO2, ZnO, Cs2CO3, SrO, PbBr2, PbCl2, NaBr, NaCl, and Al2O3.

[0016] Preferably, in step (1), the total molar percentage of B2O3, SiO2, ZnO, Cs2CO3, SrO, PbBr2, PbCl2, NaBr, NaCl and Al2O3 is 100%, wherein the molar percentage of B2O3 is 25%-45%, the molar percentage of SiO2 is 10%-35%, the molar percentage of ZnO is 7%-15%, the molar percentage of Cs2CO3 is 5%-13%, the molar percentage of SrO is 4%-8%, the molar percentage of PbBr2 is 3%-6%, the molar percentage of PbCl2 is 2%-6%, the molar percentage of NaBr is 2%-6%, the molar percentage of NaCl is 2%-7% of the total elements, and the molar percentage of Al2O3 is 1%-3%.

[0017] Preferably, the calcination conditions in step (1) are: calcination at 1150-1300° for 12-25 min in an air atmosphere.

[0018] Preferably, the preheating temperature of the copper plate mold in step (2) is: 280-380°C.

[0019] The CsPbCl2Br quantum dots prepared by the method of the present invention have luminescence characteristics in the visible light and near-infrared regions.

[0020] Beneficial Effects of the Invention

[0021] (1) The present invention makes it easy to precipitate CsPbCl2Br1 quantum dots on a glass substrate by adding rare earth oxides.

[0022] (2) The present invention successfully prepared stable CsPbCl2Br1 quantum dot glass by adding rare earth oxides. The CsPbCl2Br1 perovskite prepared by the present invention has a wide light emission range and can be adjusted to different colors, such as blue to green light, which gives it certain advantages in display technology and optoelectronic devices.

[0023] (3) The prepared CsPbCl2Br1 perovskite usually performs well in terms of environmental stability. The mixture of chlorine and bromine can improve the chemical stability of the material and reduce the degradation of the material in air and humidity.

[0024] (4) The two rare earth oxides Nd2O3 or Er2O3 selected in the present invention have a better precipitation effect on CsPbCl2Br quantum dots in glass, and have better luminescence in the near-infrared region, and can achieve luminescence modes in the visible region and near-infrared region. Rare earth doping can further expand the optical properties of perovskite quantum dots, enabling them to achieve efficient luminescence in the near-infrared band, meeting the needs of optical communications, imaging, night vision equipment and security detection, and the doping of the two rare earth oxides can reduce the photodegradation phenomenon of CsPbCl2Br1 quantum dot glass.

[0025] (5) Through a specific process flow, the rare earth-doped perovskite quantum dots are uniformly dispersed in the glass matrix, thereby improving the overall performance of the material and avoiding the performance degradation caused by uneven dispersion of quantum dots. The glass matrix itself has excellent mechanical strength and chemical stability, which further enhances the durability of the composite material, allowing it to maintain stable optical and physical properties under harsh environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is the XRD pattern of the perovskite quantum dot glass prepared in Example 1.

[0027] Figure 2 This is the TEM image of the perovskite quantum dot glass prepared in Example 1.

[0028] Figure 3 This is a particle size diagram of the perovskite quantum dot glass prepared in Example 1.

[0029] Figure 4 This is the photoluminescence (PL) spectrum of the perovskite quantum dot glass prepared in Example 1 in the visible and near-infrared.

[0030] Figure 5 This is the photoluminescence (PL) spectrum of the perovskite quantum dot glass prepared in Example 2 in the visible and near-infrared.

[0031] Figure 6 Photo of the imaging application of the perovskite quantum dot glass prepared for implementation case 1 in the near-infrared region. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0033] Example 1

[0034] A CsPbCl2Br1NCs perovskite quantum dot glass comprises the following raw materials in molar percentage: 37% B2O3, 28% SiO2, 9% ZnO, 5% SrO, 7% Cs2CO3, 4% PbBr2, 2% PbCl2, 2% NaBr, 4% NaCl, 2% Al2O3, wherein the molar percentage of Nd2O3 added is 3% of the total amount of B2O3, SiO2, ZnO, Cs2CO3, SrO, PbBr2, PbCl2, NaBr, NaCl, and Al2O3.

[0035] The method for preparing the perovskite quantum dot glass comprises the following steps:

[0036] (1) 10 g of perovskite quantum dot glass raw material was fully ground for more than 15 minutes, and then the ground material was transferred to an alumina crucible. The crucible containing the material was then placed in a box muffle furnace, the temperature was set to 1200° C., and the sintering time was 15 minutes to obtain a glass melt.

[0037] (2) The glass melt obtained in step (1) is taken out from the box-type muffle furnace, poured into a copper plate mold preheated to 350° C., and rapidly cooled to form and crystallize to obtain Nd-doped CsPbCl2Br perovskite quantum dot glass.

[0038] Nd 3+ Doping can produce luminescence peaks in the near-infrared region (such as 880nm, 1060nm and 1330nm). Nd-doped CsPbBrCl2 perovskite quantum dot glass exhibits excellent optical properties in the near-infrared region, giving it broad application prospects in multiple high-tech fields.

[0039] according to Figure 1 , it was found that in the XRD spectrum, after analyzing the diffraction peaks, the diffraction peak corresponding to the perovskite was located between CsPbBr3 and CsPbCl3. Compared with the standard PDF card of CsPbCl3, its diffraction peak was slightly shifted to a small angle, which indicated that part of the Br element entered the interior of CsPbCl3, replacing the position of Cl, resulting in lattice expansion, which further proved the formation of CsPbCl2Br1 type mixed halogen perovskite quantum dots.

[0040] according to Figure 2 Through transmission electron microscopy (TEM) observation, it can be seen that the white part in the image is the glass matrix, while the black part is the CsPbCl2Br1 type mixed halogen perovskite quantum dots. The TEM image also clearly shows the lattice fringes, which further verifies that the introduction of rare earth doping in the implementation case can induce the formation of CsPbCl2Br1 quantum dots in the glass matrix.

[0041] according to Figure 3By measuring the grain size, the result of 3.88nm was obtained, which is consistent with the size of CsPbCl2Br1 perovskite quantum dots, indicating that CsPbCl2Br1 quantum dots were successfully precipitated in the glass; this result was measured by using transmission electron microscopy (TEM) and other techniques, verifying that the size of the quantum dots in the experiment was consistent with expectations.

[0042] CsPbCl2Br1 perovskite quantum dots have excellent photoelectric properties, and their precipitation process in the glass matrix may involve solution treatment, heat treatment and other methods; this data not only verifies the reliability of material preparation, but also provides a basis for further research on the stability and application performance of quantum dots in glass.

[0043] according to Figure 4 , by measuring under 365nm laser excitation, the luminescence phenomenon of CsPbCl2Br1 quantum dots at 448nm was observed ( Figure 4 (A)), and at the same time, under 980nm laser excitation, near-infrared light emission in the 1060nm region was detected ( Figure 4 (B)); This result demonstrates that CsPbCl2Br1 quantum dots have broad application potential in the visible and near-infrared regions.

[0044] according to Figure 6 , further demonstrating the application prospects of near-infrared LEDs in night market lighting; the figure includes color and black-and-white photos of natural light and when the LED is turned on, these images can be clearly captured by visible light cameras and near-infrared cameras; this shows that near-infrared LEDs have the potential to be used as imaging light sources, especially in imaging applications.

[0045] Example 2

[0046] A CsPbCl2Br1NCs perovskite quantum dot glass comprises the following raw materials in molar percentage: 39% B2O3, 34% SiO2, 7% ZnO, 4% SrO, 5% Cs2CO3, 3% PbBr2, 2% PbCl2, 2% NaBr, 2% NaCl, 2% Al2O3, and the molar percentage of Er2O3 added is 20% of the total amount of B2O3, SiO2, ZnO, Cs2CO3, SrO, PbBr2, PbCl2, NaBr, NaCl, and Al2O3.

[0047] The method for preparing the perovskite quantum dot glass comprises the following steps:

[0048] (1) 10 g of perovskite quantum dot glass raw material was fully ground for more than 15 minutes, and then the ground material was transferred to an alumina crucible; then the crucible containing the material was placed in a box muffle furnace, the temperature was set to 1200° C., and the sintering time was 15 minutes to obtain a glass melt.

[0049] (2) The glass melt obtained in step (1) is taken out from the box-type muffle furnace, poured into a copper plate mold preheated to 350° C., and rapidly cooled to form and crystallize to obtain Er-doped CsPbCl2Br1 perovskite quantum dot glass.

[0050] according to Figure 5 , the luminescence phenomenon of CsPbCl2Br1 quantum dots was observed by measuring under 365nm laser excitation ( Figure 5 (A)), and at the same time, under 808nm laser excitation, near-infrared broadband emission in the 1535nm region was detected ( Figure 5 (B)). This result proves that CsPbCl2Br1 quantum dots have broad application potential in the visible and near-infrared regions, demonstrating their diversity and application prospects in different spectral regions.

[0051] Erbium-doped perovskite quantum dot glass materials have unique absorption and emission characteristics in the near-infrared region. 3+ ) after the material has been treated with a laser, a characteristic optical emission peak will appear near 1.54μm (1535nm), which makes it potentially applicable in the optical communication band.

[0052] Comparative Example 1

[0053] A CsPbCl2Br1NCs perovskite quantum dot glass comprises raw materials with the following molar percentages: 37% B2O3, 28% SiO2, 9% ZnO, 5% SrO, 7% Cs2CO3, 4% PbBr2, 2% PbCl2, 2% NaBr, 4% NaCl, 2% Al2O3, and Sm2O3. The molar percentage of added Sm2O3 is 3% of the total amount of B2O3, SiO2, ZnO, Cs2CO3, SrO, PbBr2, PbCl2, NaBr, NaCl, and Al2O3.

[0054] The method for preparing the perovskite quantum dot glass comprises the following steps:

[0055] (1) 10 g of perovskite quantum dot glass raw material was fully ground for more than 15 minutes, and then the ground material was transferred to an alumina crucible. The crucible containing the material was then placed in a chamber muffle furnace, the temperature was set to 1200° C., and the sintering time was 15 minutes.

[0056] (2) The glass melt obtained in step (1) is taken out from the box-type muffle furnace, poured into a copper plate mold preheated to 350° C., and rapidly cooled to form and crystallize to obtain perovskite quantum dot glass.

[0057] Although the prepared CsPbCl2Br1NCs perovskite quantum dot glass can be obtained by rare earth induced self-crystallization, the luminescence of the rare earth Sm is around 595nm and will not emit light in the near-infrared region, which restricts its application in the near-infrared region and cannot be used in near-infrared applications.

[0058] Comparative Example 2

[0059] A CsPbCl2Br1NCs perovskite quantum dot glass comprises the following raw materials in molar percentage: 37% B2O3, 28% SiO2, 9% ZnO, 5% SrO, 7% Cs2CO3, 4% PbBr2, 2% PbCl2, 2% NaBr, 4% NaCl, 2% Al2O3, and Eu2O3. The molar percentage of added B2O3 is 3% of the total amount of B2O3, SiO2, ZnO, Cs2CO3, SrO, PbBr2, PbCl2, NaBr, NaCl, and Al2O3.

[0060] The method for preparing the perovskite quantum dot glass comprises the following steps:

[0061] (1) 10 g of perovskite quantum dot glass raw material was fully ground for more than 15 minutes, and then the ground material was transferred to an alumina crucible. The crucible containing the material was then placed in a chamber muffle furnace, the temperature was set to 1200° C., and the sintering time was 15 minutes.

[0062] (2) The glass melt obtained in step (1) is taken out from the box-type muffle furnace, poured into a copper plate mold preheated to 350° C., and rapidly cooled to form and crystallize to obtain perovskite quantum dot glass.

[0063] Although CsPbCl2Br1NCs perovskite quantum dot glass can be prepared by rare earth induced self-crystallization technology, the luminescence of the rare earth element Eu is mainly concentrated around 620nm, which limits its application in the near-infrared region and is therefore not suitable for near-infrared related application scenarios.

Claims

1. A method for preparing a perovskite quantum dot dual-spectrum luminescent glass material, characterized in that: The preparation method specifically comprises the following steps: (1) High-purity B2O3, SiO2, ZnO, Cs2CO3, SrO, PbBr2, PbCl2, NaBr, NaCl, Al2O3 and rare earth oxides are fully mixed and ground, and then calcined to obtain a glass melt; the rare earth oxide is one of Nd2O3 and Er2O3; (2) Pour the glass melt obtained in step (1) into a preheated copper plate mold, cool it naturally and form it, so as to obtain CsPbCl2Br1NCs perovskite quantum dot glass, which is a perovskite quantum dot dual-spectrum luminescent glass material.

2. The method for preparing the perovskite quantum dot dual-spectrum luminescent glass material according to claim 1, characterized in that: The molar percentage of the rare earth element added in step (1) is 1%-10% of the total amount of B2O3, SiO2, ZnO, Cs2CO3, SrO, PbBr2, PbCl2, NaBr, NaCl, and Al2O3.

3. The method for preparing the perovskite quantum dot dual-spectrum luminescent glass material according to claim 1, characterized in that: In step (1), the total molar percentage of B2O3, SiO2, ZnO, Cs2CO3, SrO, PbBr2, PbCl2, NaBr, NaCl and Al2O3 is 100%, wherein the molar percentage of B2O3 is 25%-45%, the molar percentage of SiO2 is 10%-35%, the molar percentage of ZnO is 7%-15%, the molar percentage of Cs2CO3 is 5%-13%, the molar percentage of SrO is 4%-8%, the molar percentage of PbBr2 is 3%-6%, the molar percentage of PbCl2 is 2%-6%, the molar percentage of NaBr is 2%-6%, the molar percentage of NaCl is 2%-7% of the total elements and the molar percentage of Al2O3 is 1%-3%.

4. The method for preparing the perovskite quantum dot dual-spectrum luminescent glass material according to claim 1, characterized in that: The calcination conditions in step (1) are: calcination at 1150-1300°C for 12-25 min in an air atmosphere.

5. The method for preparing the perovskite quantum dot dual-spectrum luminescent glass material according to claim 1, characterized in that: The preheating temperature of the copper plate mold in step (2) is: 280-380°C.

6. The CsPbCl2Br1 quantum dot glass prepared by the method according to any one of claims 1 to 5, characterized in that: CsPbCl2Br quantum dots have luminescence properties in the visible and near-infrared regions.

Citation Information

Patent Citations

  • Ti<4+>-doped CsPbCl2Br1 quantum dot microcrystalline glass and application thereof

    CN111302635A

Cited By

  • Cesium lead halide perovskite quantum dot glass optical fiber and preparation method thereof

    CN119661086A

  • A cesium lead halide perovskite quantum dot glass optical fiber and its preparation method

    CN119661086B