Ultraviolet-proof thermal insulation glass and preparation method thereof
By using multi-layer structure and gradient distribution of squid cellulose in UV-proof glass, combined with thermoplastic hot melt resin and air-curing resin, the problem of low compressive strength of UV-proof glass in the prior art is solved, and good insulation is achieved UV resistance.
Patent Information
- Application Number
- CN202411096862.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-12
AI Technical Summary
When existing UV-proof glass improves insulation performance, its compressive strength is low, making it difficult to take into account both insulation effect and compressive performance.
UV insulation glass with a multi-layer structure, the first glass layer contains butyroxate formamide phenylethanol, chloroacetone o-hydroxybenzamidine and sea squid cellulose, and the second glass layer contains glass powder and trisphenyl phosphate Dicarboxylate ethoxysilane) ester and aluminum glycine, the bonding layer contains thermoplastic hot melt resin and air-curing resin. Through the gradient distribution of the sea squid cellulose and the design of the bonding layer, the UV resistance and compressive resistance are enhanced.
It significantly improves the UV resistance and insulation performance of glass, while also improving compressive strength, avoiding the reduction of insulation and compression performance.
Smart Images

Figure CN118930075A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of anti-ultraviolet thermal insulation glass, and in particular to an anti-ultraviolet thermal insulation glass and a preparation method thereof. Background Art
[0002] Glass is the most common material in our daily life and is closely related to people's production activities. With the development of modern science and technology, glass technology and the improvement of people's living standards, the function of architectural glass is no longer just to meet the lighting requirements, but also to have the characteristics of light regulation, thermal insulation, bulletproof, anti-theft, fire prevention, radiation protection, anti-electromagnetic interference, artistic decoration, etc.
[0003] In recent years, in order to improve the thermal insulation performance of glass, vacuum glass is prepared by sealing two pieces of flat glass on all sides, evacuating the gap between them and sealing the exhaust holes. The gap between the two pieces of glass is 0.1-0.2 mm. However, this will make the thermal insulation glass thicker, which consumes manpower and material resources during installation, and often affects the overall aesthetics of the home after installation. Subsequently, porous thermal insulation glass came into being. Porous thermal insulation glass is prepared by forming a large number of channels in the glass through acid immersion or alkali immersion, but it will cause the compressive strength of the glass to drop sharply.
[0004] In view of this, how to obtain an anti-ultraviolet glass with good thermal insulation and good compressive strength has become the focus of the current glass manufacturing industry. Summary of the invention
[0005] The embodiment of the present application provides an anti-ultraviolet thermal insulation glass and a preparation method thereof, which are used to solve the technical problems of poor thermal insulation effect and low compressive strength of the anti-ultraviolet glass in the prior art.
[0006] In a first aspect, an embodiment of the present application provides an anti-ultraviolet thermal insulation glass, the anti-ultraviolet thermal insulation glass comprising: the anti-ultraviolet thermal insulation glass comprising: a first glass layer (11, 15) and a second glass layer (13), and an adhesive layer (12, 14);
[0007] The first glass layer (11, 15) comprises butyric acid carboxamidophenylethanol, chloroacetonyl o-hydroxybenzamide and ascidian cellulose;
[0008] The second glass layer (13) comprises glass powder, tri(phthaloethoxysilane) phosphate and aluminum glycinate;
[0009] The bonding layer (12, 14) comprises a thermoplastic hot melt resin and an air curing resin having a melting temperature of 60 to 120°C;
[0010] The content of the thermoplastic hot-melt resin accounts for 20 to 80% of the total weight of the bonding layer; the content of the air-curing resin accounts for 10 to 40% of the total weight of the bonding layer.
[0011] In a possible implementation manner, the content ratio of the ascidian cellulose in the first glass layer (11, 15) to the first glass layer, and the content ratio on the side close to the second glass layer (13) is less than or equal to 20%;
[0012] The content ratio of the ascidian cellulose in the first glass layer (11, 15) to the first glass layer is greater than or equal to 60% on the side away from the second glass layer (13).
[0013] In a possible implementation manner, the content ratio of ascidian cellulose in the first glass layer (11, 15) increases gradually from close to the second glass layer (13) to far away from the second glass layer (13).
[0014] In a possible implementation manner, the thickness of the second glass layer (13) does not exceed 0.3 mm;
[0015] The thickness of the bonding layer (12, 14) does not exceed 0.1 mm;
[0016] The thickness of the first glass layer (11, 15) does not exceed 3 mm.
[0017] In a possible implementation, the thermoplastic hot melt resin includes: one or more of polyvinyl acetate polyamide, hydrocarbon resin, asphalt, tar, wax, paraffin, raw rubber, fluorinated rubber, polyvinyl chloride, polyamide, fluorocarbon or polystyrene in any proportion;
[0018] The air-curing resin includes any one of alkoxysilane-terminated polyurethane, alkoxysilane-terminated polyether, polydimethylsiloxane resin or organic functional silane.
[0019] In a second aspect, an embodiment of the present application provides a method for preparing an ultraviolet-proof thermal insulation glass, the preparation method comprising:
[0020] Tri(phthaloylethoxysilyl)phosphate and aluminum glycinate are added to an ethanol and aqueous solution in a volume ratio of 7:3, respectively, and stirred, the pH value is adjusted to alkaline, and an organic solvent is added at a temperature below 0°C under inert gas protection;
[0021] Adding glass powder to the mixed solution, stirring rapidly for 1 to 8 hours, placing in a crucible, heating to above 200° C., cooling and washing, to obtain the second glass layer;
[0022] Adding butyric acid carboxamidophenylethanol and chloroacetone o-hydroxybenzamide to dimethyl sulfoxide in a mass ratio of 1:0.55-0.65 and stirring, adding rubidium chloride and cesium carbonate to adjust the pH to neutral, adding the seabridge cellulose solution, and heating to 90-110° C. to obtain a first glass liquid;
[0023] The bonding liquid is scraped onto the surface of the second glass layer, and after drying and curing at 60-90°C, a bonding layer is formed. A certain thickness of the first glass liquid is coated on the bonding layer, and the layer is placed at -5°C to 0°C for 1 to 10 hours. After being taken out, the layer is dried at no more than 90°C to obtain the UV-proof thermal insulation glass.
[0024] Further, in an optional embodiment, the mass ratio of tri(phthalylethoxysilane) phosphate and aluminum glycinate is (1-3): (2.5-8.2);
[0025] The mass ratio of tri(phthaloylethoxysilane) phosphate to glass powder is (0.1-0.2):(0.001-0.02).
[0026] Further, in an optional embodiment, the adjusting the pH value to alkaline includes adding sodium hydroxide or potassium hydroxide to adjust the pH value to between 8.5 and 10.2;
[0027] The temperature below 0°C includes -30 to -2°C;
[0028] The inert gas includes any one of nitrogen, helium, or argon;
[0029] The heating temperature in the crucible is 150-400° C.
[0030] The organic solvent includes N,N-dimethylformamide or N,N-dimethylacetamide.
[0031] Further, in an optional embodiment, the mass volume ratio of the butyric acid carboxamidophenylethanol and dimethyl sulfoxide is (1-3) g: (5-50) mL.
[0032] Further, in an optional embodiment, the mass ratio of the butyric acid carboxamidophenylethanol and rubidium chloride is (0.1-1): (0.0001-0.0018).
[0033] The anti-ultraviolet thermal insulation glass and the preparation method thereof provided in the embodiments of the present application have the following beneficial effects compared with the prior art:
[0034] 1. The anti-ultraviolet thermal insulation glass of the present application adopts a multi-layer, in which sea squirt cellulose is added to the anti-ultraviolet layer. Due to the anti-ultraviolet performance of sea squirt cellulose, after hydrolysis with butyric acid formamidophenylethanol, o-hydroxyphenyl triazine compounds are formed for synergistic effect, thereby enhancing the anti-ultraviolet performance of the thermal insulation glass of the present application; at the same time, the infrared absorption performance of sea squirt cellulose improves the thermal insulation performance of the glass through the synergistic effect of absorbing light energy with o-hydroxyphenyl triazine compounds.
[0035] 2. The anti-ultraviolet layer in the present application is made by adding ascidian cellulose and controlling the growth of the fiber crystals through low-temperature freeze-thaw. When exposed to sunlight, the fiber crystals can transfer the heat energy on the surface to the insulation layer in the middle layer, and under the protection of the polymer bonding layer, the heat in the second glass layer is easily absorbed but not easily diffused, thereby further improving its insulation performance.
[0036] 3. In the present application, the anti-ultraviolet layer adopts the method of adding cellulose in an increasing amount from the inside to the outside surface, mainly because the outermost surface of the anti-ultraviolet thermal insulation glass has a high cellulose content of cellulose, and its fiber crystals can protect against ultraviolet rays under synergistic conditions, and at the same time absorb heat and transfer the heat to the bonding layer and the second glass layer, while the content is lower on the side close to the bonding layer, which prevents the heat absorbed to the second glass layer from being transferred out through a high proportion of fiber crystals; by controlling the content of cellulose from close to the second glass layer to the outer surface, the anti-ultraviolet performance can be greatly improved, and while increasing the heat absorbed by the glass, it can also prevent heat from diffusing from the inside.
[0037] 4. By adding ascidian cellulose and a bonding layer, fiber crystals are formed on the outer layer, which can synergistically improve the compressive resistance of the UV-proof thermal insulation glass, making it less likely to be damaged by pressure. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0039] Figure 1 A schematic diagram of the structure of an anti-ultraviolet thermal insulation glass provided in an embodiment of the present application;
[0040] Figure 2 A flow chart of a method for preparing UV-proof thermal insulation glass provided in an embodiment of the present application.
[0041] The above drawings have shown clear embodiments of the present application, which will be described in more detail later. These drawings and text descriptions are not intended to limit the scope of the present application in any way, but to illustrate the concept of the present application to those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION
[0042] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The implementations described in the following exemplary embodiments do not represent all implementations consistent with the present application. Instead, they are merely examples of devices and methods consistent with some aspects of the present application as detailed in the appended claims.
[0043] First, the terms involved in this application are explained:
[0044] Glass powder: It is an inorganic amorphous hard particle powder, usually used as a high-transparency and high-hardness filling material. The raw materials used in production are PbO, SiO2, TiO2 and other electronic-grade raw materials, which are mixed and then reacted at high temperature to form a disordered glass homogeneous body. It has stable chemical properties and its acid resistance far exceeds that of lead oxide. However, in the expression of chemical composition, it is usually converted into oxides, such as PbO, SiO2, etc.
[0045] In recent years, in order to improve the thermal insulation performance of glass, vacuum glass is prepared by sealing two pieces of flat glass on all sides, evacuating the gap between them and sealing the exhaust holes. The gap between the two pieces of glass is 0.1-0.2 mm. However, this will make the thermal insulation glass thicker, which consumes manpower and material resources during installation, and often affects the overall aesthetics of the home after installation. Subsequently, porous thermal insulation glass came into being. Porous thermal insulation glass is prepared by forming a large number of channels in the glass through acid immersion or alkali immersion, but it will cause the compressive strength of the glass to drop sharply.
[0046] Therefore, when the existing glass improves its UV protection performance, its thermal insulation performance and compressive strength will be reduced, and it is not possible to effectively take into account all three, so that the UV protection performance, thermal insulation performance and compressive strength can all reach an excellent state.
[0047] The present application provides an anti-ultraviolet thermal insulation glass and a preparation method thereof, aiming to solve the technical problems of poor thermal insulation effect and low compressive strength of the anti-ultraviolet glass in the prior art.
[0048] The technical solution of the present application and how the technical solution of the present application solves the above-mentioned technical problems are described in detail below with specific embodiments. The following specific embodiments can be combined with each other, and the same or similar concepts or processes may not be repeated in some embodiments. The embodiments of the present application will be described below in conjunction with the accompanying drawings.
[0049] In the present application, the dissolution of the seabridge cellulose is carried out by but not limited to the following methods:
[0050] The ascidian cysts are cleaned, immersed in a NaOH solution with a mass fraction for a period of time, washed with clean water, added to glacial acetic acid and sodium hypochlorite with a volume ratio of 1:2, and appropriate water is added, stirred and reacted at a temperature not higher than 100° C. for a period of time, taken out, washed, and dried to obtain ascidian cellulose;
[0051] The sea squirt cellulose is added to a mixed solution of urea, sodium hydroxide and water, placed at -20 to -12°C for a period of time, and then stirred at room temperature. After repeated steps, a sea squirt cellulose solution is obtained.
[0052] The glass powder in the present application includes one or more of any proportion of cullet, lead tetroxide, zirconium oxide, lime, SiO2, TiO2, etc., and can be obtained, for example, by the following method:
[0053] Mix broken glass, lead tetroxide, zirconium oxide, lime, SiO2 and TiO2 in a mass ratio of 1:0.5:0.1:0.15:1:0.7, stir at 300r / min for 30min, bake at 50℃ for 2h, ball-mill in a ball mill for 25h, pass through a 200-mesh sieve, put into a quartz crucible, heat to 500℃ in a box-type resistance furnace, keep warm for 2h, heat to 750℃, keep warm for 3h, take out and quickly pour into 15℃ cold water to cool for 50min, then bake at 60℃ for 2h, put into a ball mill for 20h, pass through a 200-mesh sieve to obtain glass powder.
[0054] The embodiment of the present application provides an anti-ultraviolet thermal insulation glass, such as Figure 1 As shown, the anti-ultraviolet thermal insulation glass comprises: a first glass layer 11, 15 and a second glass layer 13, and bonding layers 12, 14;
[0055] The first glass layers 11, 15 include butyric acid carboxamidophenylethanol, chloroacetonyl o-hydroxybenzamide and sea squirt cellulose; the second glass layer 13 includes glass powder, tris(phthalylethoxysilane) phosphate and aluminum glycinate; the adhesive layers 12, 14 include thermoplastic hot melt resin with a melting temperature of 60 to 120° C. and air-curing resin;
[0056] The content of the thermoplastic hot-melt resin accounts for 20 to 80% of the total weight of the adhesive layer; the content of the air-curing resin accounts for 10 to 40% of the total weight of the adhesive layer.
[0057] The content ratio of the ascidian cellulose in the first glass layer 11, 15 to the first glass layer is less than or equal to 20% on the side close to the second glass layer 13; the content ratio of the ascidian cellulose in the first glass layer 11, 15 to the first glass layer is greater than or equal to 60% on the side away from the second glass layer 13;
[0058] The content ratio of ascidian cellulose in the first glass layers 11 , 15 increases gradually from close to the second glass layer 13 to far away from the second glass layer 13 .
[0059] The increase in the cellulose content of the ascidian in the embodiments of the present application can be a linear increase or a nonlinear increase. For example, with the near-bonding layer as the horizontal plane, as the thickness of the first glass layer increases, the cellulose content of the ascidian also increases. The increase includes but is not limited to that for every micron increase in thickness, the amount of increase in the cellulose content of the ascidian is 2% to 6% of the cellulose content of the ascidian in the previous thickness.
[0060] The thickness of the second glass layer 13 does not exceed 0.3 mm; the thickness of the adhesive layers 12 and 14 does not exceed 0.1 mm; and the thickness of the first glass layers 11 and 15 does not exceed 3 mm.
[0061] Thermoplastic hot melt resins include: one or more of polyvinyl acetate polyamide, hydrocarbon resin, asphalt, tar, wax, paraffin, raw rubber, fluorinated rubber, polyvinyl chloride, polyamide, fluorocarbon or polystyrene in any proportion;
[0062] The air-curing resin includes any one of alkoxysilane-terminated polyurethanes, alkoxysilane-terminated polyethers, polydimethylsiloxane resins or organofunctional silanes.
[0063] The present application provides a method for preparing an ultraviolet-proof thermal insulation glass. Figure 2 As shown, the method includes:
[0064] S201, adding tri(phthalylethoxysilyl) phosphate and aluminum glycinate to an ethanol and aqueous solution in a volume ratio of 7:3 respectively, stirring, adjusting the pH value to alkaline, and adding an organic solvent at a temperature below 0° C. under inert gas protection;
[0065] S202, adding glass powder to the above-mentioned mixed solution, stirring rapidly for 1 to 8 hours, placing in a crucible, heating to above 200° C., cooling and washing, to obtain a second glass layer;
[0066] S203, adding butyric acid carboxamidophenylethanol and chloroacetone o-hydroxybenzamide to dimethyl sulfoxide in a mass ratio of 1:0.55-0.65 and stirring, adding rubidium chloride and cesium carbonate to adjust the pH to neutral, adding hexachlorocellulose solution, and heating to 90-110° C. to obtain a first glass liquid;
[0067] S204, scrape the bonding liquid onto the surface of the second glass layer, dry and solidify at 60-90°C to form a bonding layer, apply a certain thickness of the first glass liquid on the bonding layer, place it at -5°C to 0°C for 1 to 10 hours, take it out and dry it at no more than 90°C to obtain UV-proof thermal insulation glass.
[0068] Furthermore, through the preparation method provided in the above embodiment, and the anti-ultraviolet glass provided in the embodiment, the following embodiments 1 to 3 are specifically provided:
[0069] Example 1
[0070] S301, adding tri(phthalylethoxysilane) phosphate and aluminum glycinate to ethanol and aqueous solution in a volume ratio of 7:3 respectively, stirring, adding sodium hydroxide to adjust the pH value to alkaline, adding organic solvent N,N-dimethylacetamide under the condition of inert gas protection below 0°C; wherein the mass ratio of tri(phthalylethoxysilane) phosphate and aluminum glycinate is 3:8.2; the mass ratio of tri(phthalylethoxysilane) phosphate and glass powder is 0.1:0.02;
[0071] S302, adding glass powder to the above-mentioned mixed solution, stirring rapidly for 1 to 8 hours, placing in a crucible, heating to 300° C., cooling and washing, to obtain a second glass layer;
[0072] S303, adding butyric acid methylaminophenylethanol and chloroacetonyl o-hydroxybenzamide to dimethyl sulfoxide in a mass ratio of 1:0.55 and stirring, adding rubidium chloride and cesium carbonate to adjust the pH to neutral, adding the seabridge cellulose solution, and heating to 90-110° C. to obtain a first glass liquid; wherein the mass volume ratio of butyric acid methylaminophenylethanol and dimethyl sulfoxide is 3 g:30 mL; the mass ratio of butyric acid methylaminophenylethanol and rubidium chloride is 0.1:0.0018;
[0073] S304, scrape the adhesive liquid onto the surface of the second glass layer, dry and solidify it at 60-90°C to form an adhesive layer, apply a certain thickness of the first glass liquid on the adhesive layer, place it at -5°C to 0°C for 1 to 10 hours, take it out and dry it at no more than 90°C to obtain UV-proof thermal insulation glass.
[0074] Among them, the content ratio of the UV-proof thermal insulation glass on the side close to the second glass layer 13 is equal to 15%, and the content ratio on the side away from the second glass layer 13 is equal to 80%; the bonding layers 12, 14 are selected from polyvinyl acetate polyamide and polyvinyl chloride, which account for 75% of the total weight of the bonding layers, and alkoxysilane-terminated polyurethane, which accounts for 25% of the total weight of the bonding layers; the thickness of the second glass layer 13 is 0.11mm; the thickness of the bonding layers 12, 14 is 0.01mm; the thickness of the first glass layers 11, 15 is 2.4mm.
[0075] Example 2
[0076] The preparation method of the anti-ultraviolet thermal insulation glass in this embodiment is the same as the preparation steps in Example 1, and the only difference is that the content ratio of the anti-ultraviolet thermal insulation glass in this embodiment close to the second glass layer 13 is equal to 15%, and the content ratio on the side away from the second glass layer 13 is equal to 76%; the bonding layers 12 and 14 are selected from polyvinyl acetate polyamide and fluorinated rubber accounting for 75% of the total weight of the bonding layers, and polydimethylsiloxane resin accounting for 25% of the total weight of the bonding layers; the thickness of the second glass layer 13 is 0.11mm; the thickness of the bonding layers 12 and 14 is 0.01mm; the thickness of the first glass layers 11 and 15 is 2.4mm
[0077] Example 3
[0078] The preparation method of the anti-ultraviolet thermal insulation glass in this embodiment is the same as the preparation steps in Example 1, and the only difference is that the content ratio of the anti-ultraviolet thermal insulation glass in this embodiment close to the second glass layer 13 is equal to 20%, and the content ratio on the side away from the second glass layer 13 is equal to 60%; the bonding layers 12 and 14 are selected from polyvinyl acetate polyamide and polyamide accounting for 75% of the total weight of the bonding layer, and alkoxysilane end group polyether accounting for 25% of the total weight of the bonding layer; the thickness of the second glass layer 13 is 0.11mm; the thickness of the bonding layers 12 and 14 is 0.01mm; the thickness of the first glass layers 11 and 15 is 2.4mm
[0079] Comparative Example 1
[0080] The difference between this comparative example and Example 1 is that there is no adhesive layer in this comparative example.
[0081] Comparative Example 2
[0082] The difference between this comparative example and Example 1 is that the content of the added ascidian cellulose in the first glass layer in this comparative example does not increase progressively, and the content is always 80%.
[0083] Comparative Example 3
[0084] The difference between this comparative example and the embodiment is that in this comparative example, no ascidian cellulose is added to the first glass layer.
[0085] Comparative Example 4
[0086] The difference between this comparative example and the embodiment is that there is no adhesive layer in this comparative example and no ascidian cellulose is added to the first glass layer.
[0087] Performance Test:
[0088] 1. Compressive strength: The compressive strength of the UV-proof thermal insulation glass prepared in the embodiment and the comparative example of the same length and width was measured according to GB / T6552 standard;
[0089] 2. Thermal insulation: The thermal insulation properties of the anti-ultraviolet thermal insulation glass prepared in the embodiment and the comparative example of the same mass were measured by testing the heat transfer coefficient according to GB / 6T8484;
[0090] 3. Anti-ultraviolet performance: The anti-ultraviolet thermal insulation glass prepared in the embodiment and the comparative example of the same length and width was irradiated with 365nm ultraviolet light for 8 hours continuously, with an interval of 10 hours, and after 5 cycles, the compressive strength after ultraviolet aging was measured according to GB / T6552 standard to determine the anti-ultraviolet performance;
[0091] 4. Corrosion resistance: Take the same mass of the anti-ultraviolet thermal insulation glass prepared in the embodiment and the comparative example and mix them with 98% concentrated sulfuric acid at a mass ratio of 1:10 and soak them for 2 days. After taking them out, wash them with deionized water for 3 times, put them in a 40℃ oven for 0.5h, and cool them naturally to room temperature to obtain acid-soaked anti-ultraviolet thermal insulation glass. Weigh the mass of the acid-soaked anti-ultraviolet thermal insulation glass.
[0092] Corrosion rate = 100% × (quality of UV-proof thermal insulation glass - quality of acid-soaked UV-proof thermal insulation glass) / quality of UV-proof thermal insulation glass. The above test results are shown in Table 1.
[0093] Table 1. Test results:
[0094]
[0095] It can be seen from Table 1 that in Comparative Examples 3 and 4, since no ascidian cellulose is added, the compressive resistance before and after UV aging is reduced; and in Comparative Examples 1 and 4, since there is no adhesive layer, the thermal conductivity rate is increased, and the thermal insulation performance is reduced; in Comparative Examples 3 and 4, the corrosion resistance of the glass is low.
[0096] It should be noted that, for the aforementioned method embodiments, for the sake of simplicity, they are all expressed as a series of action combinations, but those skilled in the art should be aware that the present application is not limited by the described order of actions, because according to the present application, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all optional embodiments, and the actions and modules involved are not necessarily required by the present application.
[0097] It should be further noted that, although the various steps in the flowchart are displayed in sequence according to the indication of the arrows, these steps are not necessarily executed in sequence in the order indicated by the arrows. Unless there is a clear description in this article, the execution of these steps is not strictly limited in order, and these steps can be executed in other orders. Moreover, at least a portion of the steps in the flowchart may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but can be executed at different times, and the execution order of these sub-steps or stages is not necessarily to be carried out in sequence, but can be executed in turn or alternately with other steps or at least a portion of the sub-steps or stages of other steps.
[0098] In the above embodiments, the description of each embodiment has its own emphasis. For parts not described in detail in a certain embodiment, please refer to the relevant description of other embodiments. The technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0099] Those skilled in the art will readily appreciate other embodiments of the present application after considering the specification and practicing the invention disclosed herein. The present application is intended to cover any modification, use or adaptation of the present application, which follows the general principles of the present application and includes common knowledge or customary techniques in the art that are not disclosed in the present application. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present application are indicated by the following claims.
[0100] It should be understood that the present application is not limited to the precise structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present application is limited only by the appended claims.
Claims
1. A UV-proof thermal insulation glass, characterized in that: The anti-ultraviolet thermal insulation glass comprises: a first glass layer (11, 15), a second glass layer (13), and an adhesive layer (12, 14); The first glass layer (11, 15) comprises butyric acid carboxamidophenylethanol, chloroacetonyl o-hydroxybenzamide and ascidian cellulose; The second glass layer (13) comprises glass powder, tri(phthaloethoxysilane) phosphate and aluminum glycinate; The bonding layer (12, 14) comprises a thermoplastic hot melt resin and an air curing resin having a melting temperature of 60 to 120°C; The content of the thermoplastic hot-melt resin accounts for 20 to 80% of the total weight of the bonding layer; the content of the air-curing resin accounts for 10 to 40% of the total weight of the bonding layer.
2. The anti-ultraviolet thermal insulation glass according to claim 1, characterized in that: The content ratio of the ascidian cellulose in the first glass layer (11, 15) to the first glass layer is less than or equal to 20% at the side close to the second glass layer (13); The content ratio of the ascidian cellulose in the first glass layer (11, 15) to the first glass layer is greater than or equal to 60% on the side away from the second glass layer (13).
3. The anti-ultraviolet thermal insulation glass according to claim 1 or 2, characterized in that: The content ratio of ascidian cellulose in the first glass layer (11, 15) increases gradually from close to the second glass layer (13) to far away from the second glass layer (13).
4. The anti-ultraviolet thermal insulation glass according to claim 1 or 2, characterized in that: The thickness of the second glass layer (13) does not exceed 0.3 mm; The thickness of the bonding layer (12, 14) does not exceed 0.1 mm; The thickness of the first glass layer (11, 15) does not exceed 3 mm.
5. The anti-ultraviolet thermal insulation glass according to claim 1, characterized in that: The thermoplastic hot melt resin includes: one or more of polyvinyl acetate polyamide, hydrocarbon resin, asphalt, tar, wax, paraffin, raw rubber, fluorinated rubber, polyvinyl chloride, polyamide, fluorocarbon or polystyrene in any proportion; The air-curing resin includes any one of alkoxysilane-terminated polyurethane, alkoxysilane-terminated polyether, polydimethylsiloxane resin or organic functional silane.
6. A method for preparing UV-proof thermal insulation glass, characterized in that: The preparation method comprises: Tri(phthaloylethoxysilyl)phosphate and aluminum glycinate are added to an ethanol and aqueous solution in a volume ratio of 7:3, respectively, and stirred, the pH value is adjusted to alkaline, and an organic solvent is added at a temperature below 0°C under inert gas protection; Adding glass powder to the mixed solution, stirring rapidly for 1 to 8 hours, placing in a crucible, heating to above 200° C., cooling and washing, to obtain the second glass layer; Adding butyric acid carboxamidophenylethanol and chloroacetone o-hydroxybenzamide to dimethyl sulfoxide in a mass ratio of 1:0.55-0.65 and stirring, adding rubidium chloride and cesium carbonate to adjust the pH to neutral, adding the sea squirt cellulose solution, and heating to 90-110° C. to obtain a first glass liquid; The bonding liquid is scraped onto the surface of the second glass layer, and after drying and curing at 60-90°C, a bonding layer is formed. A certain thickness of the first glass liquid is coated on the bonding layer, and the layer is placed at -5°C to 0°C for 1 to 10 hours. After being taken out, the layer is dried at no more than 90°C to obtain the UV-proof thermal insulation glass.
7. The method for preparing the UV-proof thermal insulation glass according to claim 6, characterized in that: The mass ratio of tri(phthalylethoxysilane) phosphate to aluminum glycinate is (1-3):(2.5-8.2); The mass ratio of tri(phthaloylethoxysilane) phosphate to glass powder is (0.1-0.2):(0.001-0.02).
8. The method for preparing the UV-proof thermal insulation glass according to claim 6, characterized in that: The step of adjusting the pH value to alkaline includes adding sodium hydroxide or potassium hydroxide to adjust the pH value to between 8.5 and 10.2; The temperature below 0°C includes -30 to -2°C; The inert gas includes any one of nitrogen, helium, or argon; The heating temperature in the crucible is 150-400° C. The organic solvent includes N,N-dimethylformamide or N,N-dimethylacetamide.
9. The method for preparing the UV-proof thermal insulation glass according to claim 6, characterized in that: The mass volume ratio of the butyric acid carboxamidophenylethanol and dimethyl sulfoxide is (1-3) g: (5-50) mL.
10. The method for preparing the UV-proof thermal insulation glass according to claim 6, characterized in that: The mass ratio of the butyric acid carboxamidophenylethanol and rubidium chloride is (0.1-1): (0.0001-0.0018).
Citation Information
Patent Citations
Composition for film molding, laminate, film, sheet substrate, packing material, method for producing composition for film molding, and method for producing cellulose dispersion
CN103842452A
Preparation method of sun-proof clothing material
CN112267165A
Ultraviolet-proof thermal insulation glass and preparation method thereof
CN114956590A
Preparation method of high-barrier-property biomass mulching film material based on sea squirt cellulose
CN117186474A
Base material, optical filter, and use thereof
JP2022145519A