Mine filling cementing material and preparation method thereof
By using raw materials such as cement clinker, modified phosphogypsum calcined, anhydrous gypsum and pellet desulfurization ash, the hydration heat of mine filled cementitious materials is reduced, the compressive strength and cementing performance are improved, and the existing technology is solved The poor and high cost of underground operation environment and high cost have achieved the recycling and utilization of raw materials and environmental protection.
Patent Information
- Application Number
- CN202410941506.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing mine filled gelling materials have a difficult underground operating environment due to high hydration heat, low cementing performance and compressive strength, and high raw materials prices, which are not conducive to industrial production.
The raw materials such as anhydrite made of cement clinker, modified phosphogypsum calcined, pellet desulfurization ash and blast furnace water slag are reduced through compounding and modification treatment, and the hydration heat is improved, and the compressive strength is used to utilize industrial solid waste. Recycling and reducing costs.
It significantly improves the underground operation environment, improves cementing performance and compressive strength, reduces production costs, and realizes the recycling and environmental protection of solid waste.
Smart Images

Figure BDA0004944273950000071 
Figure BDA0004944273950000081
Abstract
Description
Technical Field
[0001] The present application relates to the field of mine filling material preparation technology, and in particular to a mine filling gelling material and a preparation method thereof. Background Art
[0002] Backfill mining is becoming more and more popular due to its advantages such as improving resource recovery rate, effectively controlling ground pressure in mining areas and protecting the ecological environment of mining areas. Cementitious backfill is to mix cementitious materials, fine aggregates such as fine sand or tailings and appropriate amount of water in a certain proportion to prepare a backfill slurry, which is then transported to the underground goaf through drilling, pipelines and other methods. The slurry forms a backfill with a certain strength in the goaf. Backfill cementitious materials, as an important component of backfill slurry, directly affect the quality of the backfill.
[0003] The existing filling cementitious materials still generally use cement as the cementitious material. For example, cement clinker is compounded with dihydrate gypsum, fly ash, blast furnace slag, limestone, and activator as the filling cementitious material for mines. However, due to the high hydration heat of the product, the temperature of the filling mine room is high and the shrinkage stress of the filling body is large, so the working environment of the underground workers is difficult, which is not conducive to safe production; the product bonding performance of the filling cementitious material obtained is average, and the compressive strength is slightly low, and the compressive stability is average; and the prices of raw materials such as fly ash, limestone, and dihydrate gypsum are gradually rising, resulting in a gradual increase in costs, which is not conducive to industrial production. Summary of the invention
[0004] In order to solve the problems of existing mine filling cementitious materials, the present application provides a mine filling cementitious material and a preparation method thereof.
[0005] The present application provides a mine filling cementitious material, which adopts the following technical solution: A mine filling cementitious material comprises the following raw materials by mass percentage: 2-6% cement clinker, 8-14% anhydrite, 3-4% pellet desulfurized ash, 76-85% blast furnace slag and 1-2% activator; the anhydrite is calcined from modified phosphogypsum.
[0006] Preferably, the following raw materials are included by mass percentage: 4% cement clinker, 10% anhydrite, 4% pellet desulfurization ash, 80% blast furnace slag, and 2% activator.
[0007] By adopting the above technical scheme, cement clinker, anhydrite, pellet desulfurization ash, blast furnace slag, and activator are compounded according to the mass ratio, which can effectively reduce the hydration heat of filling cementitious materials, greatly improve the working environment of underground workers, and the product has high cementing performance, effectively improving the compressive strength of the product; a large amount of industrial solid waste is used in the raw materials, which not only reduces the production cost, but also recycles the solid waste, effectively achieving the purpose of environmental protection. Pellet desulfurization ash mainly contains calcium compounds such as CaO, CaSO3, CaSO4, Ca(OH)2, CaCO3, etc. Its particle size is smaller than that of fly ash, and it can be filled in the pores of coarse aggregate to make the structure more dense and uniform. In addition, the addition of pellet desulfurization ash can reduce the amount of cement, thereby reducing the heat generated during the cement hydration process. The modified phosphogypsum is calcined into anhydrite, which can be used in filling cementitious materials to further improve the compressive strength and durability of the product.
[0008] Preferably, the raw materials of the anhydrite include modified phosphogypsum and sodium silicate, and the mass ratio of the two is 1:0.04-0.1.
[0009] By adopting the above technical solution, sodium silicate is added during the calcination process, and the sodium silicate reacts with the calcium sulfate in the modified phosphogypsum to generate sodium sulfate and calcium silicate, which can significantly enhance the internal structure of the anhydrite and effectively improve its compressive strength and durability.
[0010] Preferably, the raw materials of the modified phosphogypsum include phosphogypsum and a modifier, and the mass ratio of the two is 1:0.028-0.034.
[0011] Preferably, the raw materials of the modifier include calcium oxide, calcium sulfate and isocyanate in a mass ratio of 1:0.1-0.3:0.2-0.3.
[0012] By adopting the above technical scheme, calcium oxide, calcium sulfate, and isocyanate are used as modifiers to effectively remove soluble impurities such as phosphorus and fluorine in phosphogypsum, effectively improving the stability and dispersibility of phosphogypsum, thereby further improving the compressive strength and durability of the filling cementitious material.
[0013] Preferably, the activator comprises sodium hydroxide and ferrous sulfate in a mass ratio of 1:0.25-0.5.
[0014] The present application also provides a method for preparing a mine filling cementitious material, which adopts the following technical solution: A method for preparing a mine filling gelling material comprises the following steps: The raw materials of cement clinker, anhydrite, pellet desulfurization ash, blast furnace slag and activator are dried and then ground, the raw materials are weighed according to the mass ratio, and then fully mixed, and after uniform mixing, the mine filling cementitious material is obtained.
[0015] Preferably, the method for preparing anhydrite comprises the following steps: The modified phosphogypsum and sodium silicate are uniformly mixed, calcined at high temperature, and aged for 3-5 days after calcination to obtain anhydrite.
[0016] Preferably, the method for preparing the modified phosphogypsum comprises the following steps: The phosphogypsum is placed in an oven at 160-180°C and dried for 5-7 hours. The dried phosphogypsum is ground and passed through a 100-150 mesh sieve. Then calcium oxide and calcium sulfate are added and mixed evenly. Then, the mixture is subjected to high-temperature modification treatment at 200-220°C for 2-3 hours. After cooling, isocyanate is added. After high-speed stirring, the mixture is dried in an oven at 45-55°C for 1-2 days. Then, the mixture is powdered for 30-50 minutes to obtain modified phosphogypsum.
[0017] Preferably, the high temperature calcination temperature is 500-550°C and the time is 1.75-2h.
[0018] In summary, the present application includes at least one of the following beneficial technical effects: 1. The mine filling cementitious material provided in this application has a significantly reduced hydration heat of the product, and the temperature of the filling mine room is significantly reduced, which greatly improves the working environment of underground workers; 2. The cementing properties of the mine filling cementitious material provided in this application are improved, and the compressive strength after 28 days of curing reaches 3.5MPa or above; 3. The mine filling cementitious material raw material provided by this application has low cost, is conducive to solving the problem of solid waste accumulation, recycles solid waste, and effectively achieves the purpose of environmental protection. DETAILED DESCRIPTION
[0019] The present application is further described in detail below with reference to the embodiments.
[0020] Preparation Example Preparation Example 1 In this preparation example, 100 g of phosphogypsum and 2.8 g of a modifier are used; the modifier comprises 2 g of calcium oxide, 0.2 g of calcium sulfate, and 0.6 g of isocyanate.
[0021] S1. 100 g of phosphogypsum was placed in an oven at 160° C. and dried for 7 h. The dried phosphogypsum was ground in a planetary ball mill and passed through a 100-mesh sieve. Then 2 g of calcium oxide and 0.2 g of calcium sulfate were added and mixed evenly. Then, the mixture was subjected to high-temperature modification treatment at 200° C. for 3 h. After cooling, 0.6 g of isocyanate was added. After high-speed stirring, the mixture was dried in an oven at 45° C. for 2 d. Then, the mixture was ground in a planetary ball mill for 30 min to obtain modified phosphogypsum. S2. 100 g of the modified phosphogypsum prepared in S1 was evenly mixed with 4 g of sodium silicate, and then calcined at 500° C. for 2 h. After calcination, the mixture was aged for 3 days to obtain anhydrite.
[0022] Preparation Example 2 In this preparation example, 100 g of phosphogypsum and 3 g of a modifier are used; the modifier comprises 2 g of calcium oxide, 0.6 g of calcium sulfate, and 0.4 g of isocyanate.
[0023] S1. 100 g of phosphogypsum was placed in an oven at 160° C. and dried for 7 h. The dried phosphogypsum was ground in a planetary ball mill and passed through a 100-mesh sieve. Then 2 g of calcium oxide and 0.6 g of calcium sulfate were added and mixed evenly. Then, the mixture was subjected to high-temperature modification treatment at 200° C. for 3 h. After cooling, 0.4 g of isocyanate was added. After high-speed stirring, the mixture was dried in an oven at 45° C. for 2 d. Then, the mixture was ground in a planetary ball mill for 30 min to obtain modified phosphogypsum. S2. 100 g of the modified phosphogypsum prepared in S1 was evenly mixed with 4 g of sodium silicate, and then calcined at 500° C. for 2 h. After calcination, the mixture was aged for 3 days to obtain anhydrite.
[0024] Preparation Example 3 In this preparation example, 100 g of phosphogypsum and 3.4 g of a modifier are used; the modifier comprises 2.3 g of calcium oxide, 0.46 g of calcium sulfate, and 0.64 g of isocyanate.
[0025] S1. 100 g of phosphogypsum was placed in an oven at 160° C. and dried for 7 h. The dried phosphogypsum was ground in a planetary ball mill and passed through a 100-mesh sieve. Then, 2.3 g of calcium oxide and 0.46 g of calcium sulfate were added and mixed evenly. Then, the mixture was subjected to high-temperature modification treatment at 200° C. for 3 h. After cooling, 0.64 g of isocyanate was added. After high-speed stirring, the mixture was dried in an oven at 45° C. for 2 d. Then, the mixture was ground in a planetary ball mill for 30 min to obtain modified phosphogypsum. S2. 100 g of the modified phosphogypsum prepared in S1 was evenly mixed with 4 g of sodium silicate, and then calcined at 500° C. for 2 h. After calcination, the mixture was aged for 3 days to obtain anhydrite.
[0026] Preparation Example 4 In this preparation example, 100 g of phosphogypsum and 2.8 g of a modifier are used; the modifier comprises 2 g of calcium oxide, 0.2 g of calcium sulfate, and 0.6 g of isocyanate.
[0027] S1. 100 g of phosphogypsum was placed in an oven at 170 ° C and dried for 6 h. The dried phosphogypsum was ground in a planetary ball mill and passed through a 130-mesh sieve. Then 2 g of calcium oxide and 0.2 g of calcium sulfate were added and mixed evenly. Then, the mixture was subjected to high-temperature modification treatment at 210 ° C for 2.5 h. After cooling, 0.6 g of isocyanate was added. After high-speed stirring, the mixture was dried in an oven at 50 ° C for 2 d. Then, the mixture was ground in a planetary ball mill for 40 min to obtain modified phosphogypsum. S2. 100 g of the modified phosphogypsum prepared in S1 was evenly mixed with 4 g of sodium silicate, and then calcined at 500° C. for 2 h. After calcination, the mixture was aged for 3 days to obtain anhydrite.
[0028] Preparation Example 5 In this preparation example, 100 g of phosphogypsum and 2.8 g of a modifier are used; the modifier comprises 2 g of calcium oxide, 0.2 g of calcium sulfate, and 0.6 g of isocyanate.
[0029] S1. 100 g of phosphogypsum was placed in an oven at 180°C and dried for 5 h, and the dried phosphogypsum was ground in a planetary ball mill and passed through a 150-mesh sieve; then 2 g of calcium oxide and 0.2 g of calcium sulfate were added and mixed evenly, and then subjected to high-temperature modification treatment at 220°C for 2 h. After cooling, 0.6 g of isocyanate was added, and the mixture was stirred evenly at high speed and dried in an oven at 55°C for 1 day, and then ground in a planetary ball mill for 50 min to obtain modified phosphogypsum; S2. 100 g of the modified phosphogypsum prepared in S1 was evenly mixed with 4 g of sodium silicate, and then calcined at 500° C. for 2 h. After calcination, the mixture was aged for 3 days to obtain anhydrite.
[0030] Preparation Example 6 The difference between Preparation Example 6 and Preparation Example 1 is that in Preparation Example 6, the mass of the modified phosphogypsum prepared from S1 is 100 g, and the mass of the sodium silicate is 7 g.
[0031] Preparation Example 7 The difference between Preparation Example 7 and Preparation Example 1 is that in Preparation Example 7, the mass of the modified phosphogypsum prepared from S1 is 100 g, and the mass of the sodium silicate is 10 g.
[0032] Preparation Example 8 The difference between Preparation Example 8 and Preparation Example 1 is that in Preparation Example 8, the mass of the modified phosphogypsum prepared from S1 is 100 g, and the mass of the sodium silicate is 1 g.
[0033] Preparation Example 9 The difference between Preparation Example 9 and Preparation Example 1 is that in Preparation Example 9, the mass of the modified phosphogypsum prepared from S1 is 100 g, and the mass of the sodium silicate is 13 g.
[0034] Preparation Example 10 The difference between Preparation Example 10 and Preparation Example 1 is that the calcination temperature used in S2 of Preparation Example 10 is 550° C. and the calcination time is 1.75 h.
[0035] Preparation Example 11 The difference between Preparation Example 11 and Preparation Example 1 is that the calcination temperature used in S2 of Preparation Example 11 is 600° C. and the calcination time is 1.5 h.
[0036] Preparation Example 12 The difference between Preparation Example 12 and Preparation Example 1 is that the calcination temperature used in S2 of Preparation Example 12 is 450° C. and the calcination time is 2.5 h. Example
[0037] Example 1 The anhydrite used in this embodiment comes from Preparation Example 1; the activators used are sodium hydroxide and ferrous sulfate, with a mass ratio of 1:0.25.
[0038] The raw materials of cement clinker, anhydrite, pellet desulfurization ash, blast furnace slag and activator are dried and then ground. 2g of cement clinker, 8g of anhydrite, 3.5g of pellet desulfurization ash, 85g of blast furnace slag and 1.5g of activator are weighed according to the mass ratio, and then fully mixed to obtain the mine filling cementitious material after mixing evenly.
[0039] Example 2 The anhydrite used in this embodiment comes from Preparation Example 1; the activators used are sodium hydroxide and ferrous sulfate, with a mass ratio of 1:0.25.
[0040] The raw materials of cement clinker, anhydrite, pellet desulfurization ash, blast furnace slag and activator are dried and then ground. 4g of cement clinker, 10g of anhydrite, 4g of pellet desulfurization ash, 80g of blast furnace slag and 2g of activator are weighed according to the mass ratio, and then fully mixed. After mixing evenly, the mine filling cementitious material is obtained.
[0041] Example 3 The anhydrite used in this embodiment comes from Preparation Example 1; the activators used are sodium hydroxide and ferrous sulfate, with a mass ratio of 1:0.25.
[0042] The raw materials of cement clinker, anhydrite, pellet desulfurization ash, blast furnace slag and activator are dried and then ground. 6g of cement clinker, 14g of anhydrite, 3g of pellet desulfurization ash, 76g of blast furnace slag and 1g of activator are weighed according to the mass ratio, and then fully mixed to obtain the mine filling cementitious material after mixing evenly.
[0043] Example 4 The difference between Example 4 and Example 1 is that the activators used in Example 4 are sodium hydroxide and ferrous sulfate in a mass ratio of 1:0.4.
[0044] Example 5 The difference between Example 5 and Example 1 is that the activators used in Example 5 are sodium hydroxide and ferrous sulfate in a mass ratio of 1:0.5.
[0045] Example 6 The difference between Example 6 and Example 1 is that the activators used in Example 6 are sodium hydroxide and ferrous sulfate in a mass ratio of 1:0.1.
[0046] Example 7 The difference between Example 7 and Example 1 is that the activators used in Example 7 are sodium hydroxide and ferrous sulfate in a mass ratio of 1:0.7.
[0047] Example 8 The difference between Example 8 and Example 1 is that the hard gypsum used in Example 8 comes from Preparation Example 2.
[0048] Example 9 The difference between Example 9 and Example 1 is that the hard gypsum used in Example 9 comes from Preparation Example 3.
[0049] Example 10 The difference between Example 10 and Example 1 is that the hard gypsum used in Example 10 comes from Preparation Example 4.
[0050] Embodiment 11 The difference between Example 11 and Example 1 is that the hard gypsum used in Example 11 comes from Preparation Example 5.
[0051] Example 12 The difference between Example 12 and Example 1 is that the hard gypsum used in Example 12 comes from Preparation Example 6.
[0052] Embodiment 13 The difference between Example 13 and Example 1 is that the hard gypsum used in Example 13 comes from Preparation Example 7.
[0053] Embodiment 14 The difference between Example 14 and Example 1 is that the hard gypsum used in Example 14 comes from Preparation Example 8.
[0054] Embodiment 15 The difference between Example 15 and Example 1 is that the hard gypsum used in Example 15 comes from Preparation Example 9.
[0055] Example 16 The difference between Example 16 and Example 1 is that the hard gypsum used in Example 16 comes from Preparation Example 10.
[0056] Embodiment 17 The difference between Example 17 and Example 1 is that the hard gypsum used in Example 17 comes from Preparation Example 11.
[0057] Embodiment 18 The difference between Example 18 and Example 1 is that the hard gypsum used in Example 18 comes from Preparation Example 12.
[0058] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that in Comparative Example 1, the pellet desulfurization ash is replaced with fly ash.
[0059] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that in Comparative Example 2, anhydrite is replaced with uncalcined modified phosphogypsum, and the specific preparation method is as follows: Place 100g of phosphogypsum in an oven at 160℃ and dry for 7h. Grind the dried phosphogypsum in a planetary ball mill and pass it through a 100-mesh sieve. Then add 2g of calcium oxide and 0.2g of calcium sulfate and mix well. Then, perform high-temperature modification treatment at 200℃ for 3h. After cooling, add 0.6g of isocyanate, stir well at high speed, dry in an oven at 45℃ for 2d, and grind in a planetary ball mill for 30min to obtain modified phosphogypsum.
[0060] Performance testing 1. The mine filling cementitious materials obtained in Examples 1-18 and Comparative Examples 1-2 were respectively placed under standard conditions (temperature 20±2°C and relative humidity ≥95%) and cured to the test age, and their mechanical properties were tested at 7 days and 28 days. The results are shown in Table 1.
[0061] The specific test results are as follows: Table 1 Performance test results It can be seen from the test results of Table 1 that the formula of the mine filling cementitious material provided in the present application and the preparation method thereof can achieve a compressive strength of 2.0 MPa or above after 7 days of curing, and a compressive strength of 3.5 MPa or above after 28 days of curing, indicating that the mine filling cementitious material provided in the present application has high compressive strength and bonding properties.
[0062] It can be seen from the test results of Examples 1-3 that the formula of the mine filling cementitious material provided in the present application provides a mine filling cementitious material with strong compressive strength; preferably, the optimal mass ratio of the raw materials is 4% cement clinker, 10% anhydrite, 4% pellet desulfurization ash, 80% blast furnace slag, and 2% activator.
[0063] It can be seen from the test results of Examples 1, 4, 5, 6, and 7 that when the mass ratio of the activator sodium hydroxide and ferrous sulfate used in the preparation of the mine filling cementitious material in the present application is in the range of 1:0.25-0.5, the obtained mine filling cementitious material has a strong compressive strength; but when the mass ratio of sodium hydroxide and ferrous sulfate is lower than or higher than this mass ratio, the compressive strength of the obtained mine filling cementitious material decreases significantly. Therefore, the preferred mass ratio of the activator sodium hydroxide and ferrous sulfate is 1:0.25-0.5.
[0064] It can be seen from the test results of Examples 1, 8, 9, 10 and 11 that the preparation method of the modified phosphogypsum provided in the present application can effectively improve the compressive strength of the modified phosphogypsum obtained by forging at high temperature and using it in filling cementitious materials.
[0065] It can be seen from the test results of Examples 1, 12, 13, 14 and 15 that when the mass ratio of the modified phosphogypsum and sodium silicate used in the preparation of anhydrite in the present application is in the range of 1:0.04-0.1, the obtained anhydrite can be used in mine filling cementitious materials to effectively improve its compressive strength; but when the mass ratio of the modified phosphogypsum and sodium silicate is lower than or exceeds this mass ratio, the compressive strength of the obtained anhydrite is significantly reduced when used in mine filling cementitious materials. Therefore, the preferred mass ratio of the modified phosphogypsum and sodium silicate is 1:0.04-0.1.
[0066] It can be seen from the test results of Examples 1, 16, 17 and 18 that when the calcination temperature used in the preparation of anhydrite in the present application is 500-550°C and the time is 1.75-2h, the obtained anhydrite can be used in mine filling cementitious materials to effectively improve its compressive strength; but when the temperature and time are outside this range, the obtained anhydrite is used in mine filling cementitious materials, and the compressive strength is significantly reduced. Therefore, the preferred high-temperature calcination temperature is 500-550°C and the time is 1.75-2h.
[0067] It can be seen from the test results of Comparative Example 1 that when fly ash is used instead of the pellet desulfurization ash provided in this application, the obtained mine filling cementitious material is significantly reduced, indicating that the pellet desulfurization ash provided in this application can effectively improve the compressive strength of the mine filling cementitious material.
[0068] It can be seen from the test results of Comparative Example 2 that when uncalcined modified phosphogypsum is used instead of the anhydrite provided in the present application, the obtained mine filling cementitious material is significantly reduced, indicating that the anhydrite provided in the present application can effectively improve the compressive strength of the mine filling cementitious material.
[0069] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A mine filling cementitious material, characterized in that: The raw materials include the following by mass percentage: 2-6% cement clinker, 8-14% anhydrite, 3-4% pellet desulfurization ash, 76-85% blast furnace slag, and 1-2% activator; the anhydrite is calcined from modified phosphogypsum.
2. The mine filling cementitious material according to claim 1, characterized in that: The following raw materials are included by mass percentage: Cement clinker 4%, anhydrite 10%, pellet desulfurization ash 4%, blast furnace slag 80%, activator 2%.
3. A mine filling cementitious material according to claim 1 or 2, characterized in that: The raw materials of the anhydrite include modified phosphogypsum and sodium silicate, and the mass ratio of the two is 1:0.04-0.
1.
4. A mine filling cementitious material according to claim 1 or 3, characterized in that: The raw materials of the modified phosphogypsum include phosphogypsum and a modifier, and the mass ratio of the two is 1:0.028-0.
034.
5. The mine filling cementitious material according to claim 4, characterized in that: The raw materials of the modifier include calcium oxide, calcium sulfate and isocyanate, and the mass ratio is 1:0.1-0:3:0.2-0.
3.
6. The mine filling cementitious material according to claim 1, characterized in that: The activator includes sodium hydroxide and ferrous sulfate in a mass ratio of 1:0.25-0.
5.
7. A method for preparing a mine filling cementitious material according to any one of claims 1 to 6, characterized in that: The following steps are involved: The raw materials of cement clinker, anhydrite, pellet desulfurization ash, blast furnace slag and activator are dried and then ground, the raw materials are weighed according to the mass ratio, and then fully mixed, and after uniform mixing, the mine filling cementitious material is obtained.
8. The method for preparing a mine filling gelling material according to claim 7, characterized in that: The preparation method of anhydrite comprises the following steps: The modified phosphogypsum and sodium silicate are uniformly mixed, calcined at high temperature, and aged for 3-5 days after calcination to obtain anhydrite.
9. The method for preparing a mine filling gelling material according to claim 8, characterized in that: The preparation method of the modified phosphogypsum comprises the following steps: The phosphogypsum is placed in an oven at 160-180°C and dried for 5-7 hours. The dried phosphogypsum is ground and passed through a 100-150 mesh sieve. Then calcium oxide and calcium sulfate are added and mixed evenly. The mixture is then subjected to high-temperature modification treatment at 200-220°C for 2-3 hours. After cooling, isocyanate is added. The mixture is stirred evenly at high speed and dried in an oven at 45-55°C for 1-2 days. The mixture is then ground for 30-50 minutes to obtain modified phosphogypsum.