Solid-waste-based low-calcium carbon-sequestration cementing material as well as preparation method and application thereof

By controlling the chemical composition and preparation process of solid waste-based low-calcium carbon fixing gelling materials, the problems of CO2 emissions and low solid waste utilization rate of traditional silicate cement production are solved, and solid waste with high mechanical properties and high carbonization properties are achieved Basic low-calcium carbon-fixed gelling materials meet the low-carbon transformation needs of the building materials industry.

CN118930086APending Publication Date: 2024-11-12BEIJING BUILDING MATERIALS ACADEMY OF SCI RES
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411064778.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional silicate cement production leads to a large amount of CO2 emissions, and under the proportion of solid waste ingredients, the mechanical properties and degree of carbonization of low-calcium carbon cementitious materials are relatively low, making it difficult to meet the low-carbon transformation needs of the building materials industry.

Method used

By controlling the calcified chemical composition of calcium and siliceous raw materials, ensure that the molar ratio of CaO to SiO2 is 0.9~2.3, and the mass ratio of Al2O3 to SiO2 is within the range of 0.10~0.22, and calcium carbide slag, magnesium slag, and iron tailings are used. , solid waste such as molybdenum tailings, gold tailings, etc., combined with appropriate Mg and Fe content, solid waste-based low-calcium carbon fixing gelling materials with high carbonization and mechanical properties are prepared.

Benefits of technology

It significantly improves the utilization rate of solid waste and reduces resource load. The strength of carbonization can reach up to 158MPa for 24 hours, and the carbon fixation amount can reach up to 230kg CO2/t, meeting the requirements of the building materials industry for high mechanical properties and low carbon emissions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a solid-waste-based low-calcium carbon-sequestration cementing material as well as a preparation method and application thereof. The preparation raw materials of the solid waste based low-calcium carbon sequestration cementing material comprise a calcium raw material and a siliceous raw material, and the firing-based chemical components of the preparation raw materials of the solid waste based low-calcium carbon sequestration cementing material comprise 37.2 to 56.7 parts by weight of CaO, 27.1 to 42.2 parts by weight of SiO2, 4.5 to 8.9 parts by weight of Al2O3, 1.0 to 5.0 parts by weight of MgO, 1.5 to 6.0 parts by weight of Fe2O3, 0.5 to 3.0 parts by weight of K2O and 0.8 to 2.0 parts by weight of Na2O; the molar ratio of the CaO to the SiO2 is 0.9 to 2.3, and the mass ratio of the Al2O3 to the SiO2 is 0.10 to 0.22. The solid waste-based low-calcium carbon sequestration cementing material has excellent carbonization performance and mechanical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon-fixing cementitious materials, and in particular to a solid waste-based low-calcium carbon-fixing cementitious material and a preparation method and application thereof. Background Art

[0002] Traditional silicate cement production emits a large amount of CO2, which exacerbates the global greenhouse effect and further causes climate change. Low-calcium carbon-fixing cementitious materials can reduce carbon in the production process and fix carbon in the application process, and can synergistically utilize a large amount of calcium and silicon solid waste, which is one of the important measures to achieve low-carbon transformation and development in the building materials industry.

[0003] The western and northern regions of my country have rich aeolian sand reserves. my country produces a large amount of tailings every year, and its comprehensive utilization rate is still at a low level. Widely distributed iron tailings, molybdenum tailings, and gold tailings can all be used as raw materials for low-calcium carbon-fixing cementitious materials. However, when the amount of various industrial solid wastes is large, the content of impurity ions such as Al, Fe, Mg, K, and Na introduced also increases accordingly. Although the sintering temperature can be reduced according to the principle of the lowest eutectic point, it also leads to a decrease in the content of four low-calcium carbonizable silicate minerals, β-C2S, γ-C2S, C3S2, and CS, thereby affecting the carbonization degree and mechanical properties of the products. Therefore, it is urgent to develop a technology that can achieve high mechanical properties and carbon fixation while maintaining a high proportion of solid waste ingredients. Summary of the invention

[0004] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide a solid waste-based low-calcium carbon-fixing cementitious material and a preparation method and application thereof.

[0005] In a first aspect of the present invention, a solid waste-based low-calcium carbon-fixing cementitious material is provided. According to an embodiment of the present invention, the raw materials for preparing the solid waste-based low-calcium carbon-fixing cementitious material include a calcium raw material and a silicon raw material, and the calcined chemical components of the raw materials for preparing the solid waste-based low-calcium carbon-fixing cementitious material include: 37.2 to 56.7 parts by weight of CaO, 27.1 to 42.2 parts by weight of SiO2, 4.5 to 8.9 parts by weight of Al2O3, 1.0 to 5.0 parts by weight of MgO, 1.5 to 6.0 parts by weight of Fe2O3, 0.5 to 3.0 parts by weight of K2O, and 0.8 to 2.0 parts by weight of Na2O; The molar ratio of CaO to SiO2 is 0.9~2.3, and the mass ratio of Al2O3 to SiO2 is 0.10~0.22.

[0006] According to the solid waste-based low-calcium carbon-fixing cementitious material of the above embodiment of the present invention, calcium raw materials and silicon raw materials are used as raw materials for preparation. Both calcium raw materials and silicon raw materials can come from solid waste, thereby significantly improving the utilization rate of solid waste and reducing resource load. By controlling the calcined chemical composition of the raw materials for preparing the solid waste-based low-calcium carbon-fixing cementitious material within the above range, the content of high-carbonized minerals in the low-calcium carbon-fixing cementitious material is relatively high, and the gel material has excellent carbonization performance and mechanical properties. In particular, by controlling the molar ratio of CaO to SiO2 within the above range, ingredients with different calcium silicate compositions can be designed. The mass ratio of Al2O3 to SiO2 within the above range can ensure the liquid phase content and promote sintering while avoiding the production of more minerals without hydration and carbonization activity. The necessary Mg and Fe content can also play an effect on mineral modification. Therefore, the solid waste-based low-calcium carbon-fixing cementitious material has excellent mechanical properties and carbonization properties. Specifically, the solid waste-based low-calcium carbon-fixing cementitious material has a carbonization strength of up to 158 MPa after 24 hours, and a carbon fixation amount of up to 230 kgCO2 / t.

[0007] It should be noted that the carbonization of solid waste-based low-calcium carbon-fixing cementitious materials is a routine operation in the field. For example, the carbonized sample is formed at a water-solid ratio of 0.1 to 0.3 and a pressure of 1.0 to 3.0 t; the carbonization conditions are a CO2 concentration of 60% to 100% and a pressure of 0.1 to 0.3 bar. At the same time, the calcination basis of the raw materials for preparing solid waste-based low-calcium carbon-fixing cementitious materials refers to the composition ratio of the raw materials after the loss on ignition is removed by calcination. The calcination conditions can be selected by those skilled in the art according to actual conditions. For example, the calcination temperature is 925°C to 975°C, and the calcination temperature is constant, for example, the calcination time is about 1 hour to constant weight.

[0008] In some embodiments of the present invention, the calcium raw material includes at least one of carbide slag, magnesium slag, and calcium-silicon slag. Thus, solid waste can be fully utilized and resource load can be reduced.

[0009] In some embodiments of the present invention, the silicon raw material includes at least one of iron tailings, molybdenum tailings, gold tailings, and aeolian sand. Thus, solid waste can be fully utilized and resource load can be reduced.

[0010] It will be understood by those skilled in the art that the specific components of calcium raw materials and siliceous raw materials vary depending on their sources. Those skilled in the art can select specific calcium raw materials and siliceous raw materials based on actual conditions. It is only necessary that the calcined-based chemical composition of the raw materials for preparing solid waste-based low-calcium carbon-fixing cementitious materials meets the above conditions.

[0011] In a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned solid waste-based low-calcium carbon-fixing cementitious material. According to an embodiment of the present invention, the method comprises: (1) Grinding the mixed powder of calcium raw material and silicon raw material to obtain raw powder; (2) pressing the raw powder into a green compact to obtain a green compact; (3) calcining and grinding the green body to obtain a solid waste-based low-calcium carbon-fixing cementitious material.

[0012] In some embodiments of the present invention, in step (1), the residue of the raw powder on a 0.080 mm square hole sieve is less than 15%. The inventors have found that the residue of the raw powder on a 0.080 mm square hole sieve is less than 15%, which can ensure that the raw materials are fully mixed and improve the sintering effect.

[0013] In some embodiments of the present invention, in step (2), the green body has a shape including a sheet, a sphere or a column.

[0014] In some embodiments of the present invention, the sheet-like green body has a thickness of less than 15 mm.

[0015] In some embodiments of the present invention, the diameters of the spherical green body and the columnar green body are respectively not greater than 15 mm.

[0016] In some embodiments of the present invention, in step (3), the calcination temperature is 1150°C to 1300°C, and the time is 30 min to 120 min. The inventors have found that controlling the calcination temperature and time within the above range can achieve sufficient sintering, reduce free CaO and SiO2, and avoid the appearance of excessive liquid phase.

[0017] In some embodiments of the present invention, in step (3), the specific surface area of ​​the solid waste-based low-calcium carbon-fixing cementitious material is 320 m 2 / kg~450m 2 The inventors have found that when the specific surface area of ​​the solid waste-based low-calcium carbon-fixing cementitious material is within the above range, the carbonization effect can be improved.

[0018] In the third aspect of the present invention, the present invention proposes the use of the above-mentioned solid waste-based low-calcium carbon-fixing cementitious material or the solid waste-based low-calcium carbon-fixing cementitious material prepared by the above-mentioned method in the field of building materials.

[0019] The present invention has at least the following technical effects: (1) The solid waste-based low-calcium carbon-fixing cementitious material provided by the present invention adopts iron tailings, molybdenum tailings, gold tailings, aeolian sand, carbide slag, magnesium slag, silicon-calcium slag, etc., with a high solid waste blending ratio, and a full solid waste batching scheme can also be used, thereby significantly improving the utilization rate of solid waste and reducing the resource load.

[0020] (2) The solid waste-based low-calcium carbon-fixing cementitious material provided by the present invention has a high content of carbonizable minerals. Although the clinker is easier to burn when it contains Al, K, and Na impurity elements, when their content is high, it is easy to form a calcium aluminum feldspar phase in the clinker mineral phase system, which is generally considered to be a mineral without hydration activity and is difficult to obtain strength through carbonization. After reasonable regulation of Mg and Fe, the present invention can form a series of modified calcium aluminum feldspar doped with Mg (Fe). The mineral has hydration activity and provides Ca, Mg and other ions for the carbonization process. The present invention forms a combination of one or more minerals of CS, C3S2, β-C2S, γ-C2S and Mg-modified calcium aluminum feldspar, which improves the strength of the product after carbonization. At the same time, the K and Na ions of the present invention can balance the charge and increase dislocation defects in the mineral phase. Therefore, after carbonization, the strength and carbon fixation amount of the solid waste-based low-calcium carbon-fixing cementitious material of the present invention are greatly improved.

[0021] (3) The low-calcium carbon-fixing cementitious material of the present invention has excellent carbonization performance and mechanical properties. The carbonization strength after 24 hours can reach up to 158 MPa, and the carbon fixation amount can reach up to 230 kgCO2 / t. DETAILED DESCRIPTION

[0022] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0023] The preparation conditions of the carbonized samples involved in the following examples and comparative examples are as follows: the carbonized samples are formed with a water-to-solid ratio of 0.15 and a pressure of 1.0 t; the carbonization conditions are a CO2 concentration of 100% and a pressure of 0.2 bar.

[0024] Example 1

[0025] The calcium raw material used is carbide slag, and the silicon raw material uses iron tailings.

[0026] (1) The calcined chemical composition of the mixed material of the calcium raw material and the silicon raw material is as follows: CaO mass fraction 46.04, SiO2 mass fraction 35.05, Al2O3 mass fraction 5.85, MgO mass fraction 3.10, Fe2O3 mass fraction 4.99, K2O mass fraction 0.82, Na2O mass fraction 1.07, the molar ratio of CaO to SiO2 is controlled to be 1.4, the mass ratio of Al2O3 to SiO2 is controlled to be 0.17, and the mixed material of the calcium raw material and the silicon raw material is ground to a 0.080 mm square hole sieve with a sieve residue of 12%; (2) Pressing the raw material powder obtained in step (1) into sheets with a thickness of 12 mm; (3) The raw material sample of step (2) was calcined at 1200°C for 60 min, and after cooling, ground to a specific surface area of ​​380 m 2 / kg, the solid waste-based low-calcium carbon-fixing cementitious material is obtained.

[0027] According to tests, the compressive strength of the solid waste-based low-calcium carbon-fixing cementitious material of this embodiment after carbonization is 158.2 MPa, and the carbon-fixing amount is 167.3 kg / t.

[0028] Example 2

[0029] The calcium raw materials used are carbide slag and magnesium slag, and the silicon raw materials use aeolian sand.

[0030] (1) The calcined chemical composition of the mixed material of calcium raw material and silicon raw material is as follows: CaO mass fraction 49.46, SiO2 mass fraction 31.16, Al2O3 mass fraction 6.67, MgO mass fraction 2.56, Fe2O3 mass fraction 1.77, K2O mass fraction 2.26, Na2O mass fraction 1.41, the molar ratio of CaO and SiO2 is controlled to be 1.7, the mass ratio of Al2O3 to SiO2 is controlled to be 0.21, and the residue on the 0.080 mm square hole sieve is ground to 12%; (2) Pressing the raw material powder obtained in step (1) into sheets with a thickness of 12 mm; (3) The raw material sample from step (2) was calcined at 1150°C for 30 min, and after cooling, ground to a specific surface area of ​​375 m 2 / kg, the solid waste-based low-calcium carbon-fixing cementitious material is obtained.

[0031] According to tests, the compressive strength of the solid waste-based low-calcium carbon-fixing cementitious material of this embodiment after carbonization is 124.5 MPa, and the carbon fixation amount is 194.9 kg / t.

[0032] Example 3

[0033] The calcium raw materials used are carbide slag and calcium-silicon slag, and the silicon raw materials use gold tailings.

[0034] (1) The calcined chemical composition of the mixed material of calcium raw material and silicon raw material is as follows: CaO mass fraction 44.00, SiO2 mass fraction 33.68, Al2O3 mass fraction 5.51, MgO mass fraction 4.86, Fe2O3 mass fraction 4.96, K2O mass fraction 0.93, Na2O mass fraction 1.02, the molar ratio of CaO and SiO2 is controlled to be 1.4, the mass ratio of Al2O3 and SiO2 is controlled to be 0.16, and the residue on the 0.080 mm square hole sieve is ground to 13%; (2) Pressing the raw material powder obtained in step (1) into a spherical shape with a diameter of 15 mm; (3) The raw material sample from step (2) was calcined at 1150°C for 30 min, and after cooling, ground to a specific surface area of ​​350 m 2 / kg, the solid waste-based low-calcium carbon-fixing cementitious material is obtained.

[0035] According to tests, the compressive strength of the solid waste-based low-calcium carbon-fixing cementitious material of this embodiment after carbonization is 152.8 MPa, and the carbon-fixing amount is 187.1 kg / t.

[0036] Example 4

[0037] The calcium raw material used is carbide slag, and the silicon raw material uses molybdenum tailings.

[0038] (1) The calcined chemical composition of the mixed material of calcium raw material and silicon raw material is as follows: CaO mass fraction 56.70, SiO2 mass fraction 29.45, Al2O3 mass fraction 6.53, MgO mass fraction 1.21, Fe2O3 mass fraction 1.86, K2O mass fraction 1.96, Na2O mass fraction 1.32, the molar ratio of CaO and SiO2 is controlled to be 2.1, the mass ratio of Al2O3 and SiO2 is controlled to be 0.22, and the residue on the 0.080 mm square hole sieve is ground to 12%; (2) Pressing the raw material powder obtained in step (1) into a spherical shape with a diameter of 15 mm; (3) The raw material sample of step (2) was calcined at 1200°C for 30 min, and after cooling, ground to a specific surface area of ​​348 m 2 / kg, the solid waste-based low-calcium carbon-fixing cementitious material is obtained.

[0039] According to tests, the compressive strength of the solid waste-based low-calcium carbon-fixing cementitious material of this embodiment after carbonization is 64.0 MPa, and the carbon-fixing amount is 233.0 kg / t.

[0040] Example 5

[0041] The calcium raw material used is magnesium slag, and the silicon raw material uses molybdenum tailings and iron tailings.

[0042] (1) The calcined chemical composition of the mixed material of calcium raw material and silicon raw material is as follows: CaO mass fraction 46.46, SiO2 mass fraction 36.77, Al2O3 mass fraction 7.81, MgO mass fraction 3.08, Fe2O3 mass fraction 1.76, K2O mass fraction 2.52, Na2O mass fraction 1.70, the molar ratio of CaO and SiO2 is controlled to be 1.4, the mass ratio of Al2O3 and SiO2 is controlled to be 0.21, and the residue on the 0.080 mm square hole sieve is ground to 12%; (2) Pressing the raw material powder obtained in step (1) into a column with a diameter of 15 mm and a height of 30 mm; (3) The raw material sample of step (2) was calcined at 1200°C for 60 min, and after cooling, ground to a specific surface area of ​​330 m 2 / kg, the solid waste-based low-calcium carbon-fixing cementitious material is obtained.

[0043] According to tests, the compressive strength of the solid waste-based low-calcium carbon-fixing cementitious material of this embodiment after carbonization is 93.4 MPa, and the carbon-fixing amount is 177.0 kg / t.

[0044] Example 6

[0045] The calcium raw materials used are carbide slag and magnesium slag, and the silicon raw materials use molybdenum tailings.

[0046] (1) The calcined chemical composition of the mixed material of calcium raw material and silicon raw material is as follows: CaO mass fraction 53.49, SiO2 mass fraction 28.03, Al2O3 mass fraction 6.06, MgO mass fraction 2.72, Fe2O3 mass fraction 1.64, K2O mass fraction 2.02, Na2O mass fraction 1.25, the molar ratio of CaO and SiO2 is controlled to be 2.0, the mass ratio of Al2O3 to SiO2 is controlled to be 0.22, and the residue on the 0.080 mm square hole sieve is ground to 10%; (2) Pressing the raw material powder obtained in step (1) into a column with a diameter of 15 mm and a height of 30 mm; (3) The raw material sample of step (2) was calcined at 1150°C for 30 min, and after cooling, ground to a specific surface area of ​​360 m 2 / kg, the solid waste-based low-calcium carbon-fixing cementitious material is obtained.

[0047] According to tests, the compressive strength of the solid waste-based low-calcium carbon-fixing cementitious material of this embodiment after carbonization is 100.2 MPa, and the carbon-fixing amount is 211.9 kg / t.

[0048] Example 7

[0049] The calcium raw material used is carbide slag, and the silicon raw material uses iron tailings.

[0050] (1) The calcined chemical composition of the mixed material of calcium raw material and silicon raw material is as follows: CaO mass fraction 38.74, SiO2 mass fraction 39.94, Al2O3 mass fraction 6.50, MgO mass fraction 3.56, Fe2O3 mass fraction 5.72, K2O mass fraction 0.95, Na2O mass fraction 1.24, the molar ratio of CaO and SiO2 is controlled to be 1.0, the mass ratio of Al2O3 to SiO2 is controlled to be 0.16, and the residue on the 0.080 mm square hole sieve is ground to 12%; (2) Pressing the raw material powder obtained in step (1) into a sheet with a thickness of 15 mm; (3) The raw material sample from step (2) was calcined at 1200°C for 30 min, and after cooling, ground to a specific surface area of ​​350 m 2 / kg, the solid waste-based low-calcium carbon-fixing cementitious material is obtained.

[0051] According to tests, the compressive strength of the solid waste-based low-calcium carbon-fixing cementitious material of this embodiment after carbonization is 97.0 MPa, and the carbon-fixing amount is 109.8 kg / t.

[0052] Comparative Example 1

[0053] The calcium raw material used is carbide slag, and the silicon raw material uses iron tailings.

[0054] (1) The calcined chemical composition of the mixed material of calcium raw material and silicon raw material is as follows: CaO mass fraction 32.71, SiO2 mass fraction 42.31, Al2O3 mass fraction 6.77, MgO mass fraction 3.86, Fe2O3 mass fraction 6.14, K2O mass fraction 1.05, Na2O mass fraction 1.34, the molar ratio of CaO and SiO2 is controlled to be 0.8, the mass ratio of Al2O3 and SiO2 is controlled to be 0.16, and the residue on the 0.080 mm square hole sieve is ground to 14%; (2) Pressing the raw material powder obtained in step (1) into a sheet with a thickness of 15 mm; (3) The raw material sample of step (2) was calcined at 1250°C for 30 min, and after cooling, ground to a specific surface area of ​​380 m 2 / kg, the solid waste-based low-calcium carbon-fixing cementitious material is obtained.

[0055] According to tests, the compressive strength of the solid waste-based low-calcium carbon-fixing cementitious material of this embodiment after carbonization is 32.1 MPa, and the carbon fixation amount is 49.5 kg / t.

[0056] Comparative Example 2

[0057] The calcium raw material used is carbide slag, and the silicon raw material uses molybdenum tailings.

[0058] (1) The calcined chemical composition of the mixed material of calcium raw material and silicon raw material is as follows: CaO mass fraction 42.23, SiO2 mass fraction 38.82, Al2O3 mass fraction 8.94, MgO mass fraction 0.41, Fe2O3 mass fraction 2.08, K2O mass fraction 2.39, Na2O mass fraction 1.97, the molar ratio of CaO and SiO2 is controlled to be 1.2, the mass ratio of Al2O3 and SiO2 is controlled to be 0.23, and the residue on the 0.080 mm square hole sieve is ground to 12%; (2) Pressing the raw material powder obtained in step (1) into a sheet with a thickness of 15 mm; (3) The raw material sample of step (2) was calcined at 1200°C for 30 min, and after cooling, ground to a specific surface area of ​​375 m 2 / kg, the solid waste-based low-calcium carbon-fixing cementitious material is obtained.

[0059] According to tests, the compressive strength of the solid waste-based low-calcium carbon-fixing cementitious material of this embodiment after carbonization is 42.2 MPa, and the carbon fixation amount is 57.8 kg / t.

[0060] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A solid waste-based low-calcium carbon-fixing cementitious material, characterized in that: The raw materials for preparing the solid waste-based low-calcium carbon-fixing cementitious material include calcium raw materials and silicon raw materials, and the calcined chemical components of the raw materials for preparing the solid waste-based low-calcium carbon-fixing cementitious material include: 37.2-56.7 parts by weight of CaO, 27.1-42.2 parts by weight of SiO2, 4.5-8.9 parts by weight of Al2O3, 1.0-5.0 parts by weight of MgO, 1.5-6.0 parts by weight of Fe2O3, 0.5-3.0 parts by weight of K2O, and 0.8-2.0 parts by weight of Na2O; The molar ratio of CaO to SiO2 is 0.9~2.3, and the mass ratio of Al2O3 to SiO2 is 0.10~0.

22.

2. The material according to claim 1, characterized in that The calcium raw material includes at least one of carbide slag, magnesium slag and silicon-calcium slag.

3. The material according to claim 1 or 2, characterized in that: The siliceous raw material includes at least one of iron tailings, molybdenum tailings, gold tailings and aeolian sand.

4. A method for preparing the solid waste-based low-calcium carbon-fixing cementitious material according to any one of claims 1 to 3, characterized in that: include: (1) Grinding the mixture of calcium raw material and silicon raw material to obtain raw powder; (2) pressing the raw powder into a green compact to obtain a green compact; (3) calcining and grinding the green body to obtain a solid waste-based low-calcium carbon-fixing cementitious material.

5. The method according to claim 4, characterized in that: In step (1), the raw powder has a sieve residue of less than 15% on a 0.080 mm square hole sieve.

6. The method according to claim 4, characterized in that: In step (2), the green body has a shape including a sheet, a sphere or a column.

7. The method according to claim 6, characterized in that: The thickness of the sheet green body is less than 15 mm; And / or, the diameters of the spherical green body and the columnar green body are respectively not greater than 15 mm.

8. The method according to claim 4, characterized in that: In step (3), the calcination temperature is 1150°C to 1300°C, and the calcination time is 30 min to 120 min.

9. The method according to claim 4 or 8, characterized in that: In step (3), the specific surface area of ​​the solid waste-based low-calcium carbon-fixing cementitious material is 320 m 2 / kg~450m 2 / kg.

10. Use of the solid waste-based low-calcium carbon-fixing cementitious material according to any one of claims 1 to 3 or the solid waste-based low-calcium carbon-fixing cementitious material prepared by the method according to any one of claims 4 to 9 in the field of building materials.

Citation Information

Cited By

  • Mix proportion design method of solid waste cementing material considering loess characteristics