Cement activator as well as preparation method, use method and application thereof
Through the application of double-material cement activator in the raw material calcination and grinding stages, the cement crystal form and grinding efficiency are regulated, and the existing cement activator cost and CO2 emissions are solved, and the early strength and energy consumption of cement are improved. Reduced effect.
Patent Information
- Application Number
- CN202410999042.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
While the existing cement activators improve the early strength and grinding efficiency of cement, they have high costs, poor adaptability, and negative impacts on the long-term performance of cement, and it is difficult to effectively reduce CO2 emissions.
The double-material cement activator consisting of boron oxide, iron-containing barium slag, electric furnace phosphorus slag and polymer polyol are used in the raw material calcination and cement grinding stages respectively to regulate the β-C2S crystal transformation and improve grinding efficiency. Granulation with particles promotes the strength growth of cement 3D and 28D, and improves the degree of hydration and carbonization resistance through layered bimetal oxides.
On the premise of reducing the cement clinker mix ratio, increase the strength of cement 3d and 28d, reduce the energy consumption of raw materials calcination and grinding, reduce CO2 emissions, and realize a green and environmentally friendly high-efficiency and energy-saving cement activator.
Smart Images

Figure BDA0004961046670000161 
Figure BDA0004961046670000171
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cement additives, and relates to a cement activator and a preparation method, a use method and an application thereof, and specifically relates to a high-efficiency and energy-saving cement activator and a preparation method, a use method and an application thereof. Background Art
[0002] Cement refers to a powdered hydraulic inorganic cementitious material that becomes a slurry after adding water and stirring. It can harden in the air or in water and can firmly bind materials such as sand and stone together. In the cement production process, carbonate decomposition, raw material calcination, and clinker grinding will emit a large amount of CO2, which will lead to an intensified greenhouse effect and harm the natural environment.
[0003] According to the "Building Materials Industry Carbon Peak Implementation Plan", building materials companies are encouraged to use fly ash, industrial waste slag, tailings slag, etc. as raw materials or cement admixtures. However, under the premise of not affecting the engineering quality and service life of cement concrete products, when fly ash or blast furnace slag and other admixtures are used to replace clinker, the early strength of cement-based materials will be reduced because most admixtures have problems such as early activity that is difficult to activate or even cannot be activated.
[0004] Traditional cement activators are mainly used in the cement clinker grinding stage to solve the problems of cement particles agglomerating or adhering to the surface of equipment, which can effectively improve the cement grinding effect and increase the early strength of cement. This type of cement activator usually uses alcohol amine + inorganic salt as the main components. Its disadvantages are high cost, different adaptability in cement in different regions, and it is not conducive to controlling the chloride ion content in cement. It may even have a negative impact on the long-term performance of cement, such as a decrease in 28d mechanical strength and reduced concrete durability. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a cement activator and a preparation method thereof. The cement activator can improve the burnability of raw materials and reduce the coal consumption during the raw material calcination stage, and at the same time regulate the β-C2S crystal transformation to improve the early strength of cement clinker; in the cement grinding stage, it can improve the grinding efficiency of cement clinker, reduce the power consumption of grinding, optimize the particle grading, and promote the joint growth of cement 3d and 28d strengths under the premise of reducing the mix ratio of cement clinker.
[0006] The invention also provides a method for using the cement activator. The S material in the cement activator is used in the raw material grinding process, and the L material is used in the cement grinding process.
[0007] The invention also provides application of the cement activator as a cement admixture.
[0008] The technical solution adopted by the present invention is as follows:
[0009] A cement activator is composed of S material and L material. The S material comprises boron oxide, iron-barium slag and electric furnace phosphorus slag; the L material comprises polymer polyol solution, layered bimetallic oxide, industrial byproduct sodium thiocyanate solution and water.
[0010] The S material is used in the raw material grinding process; the L material is used in the cement grinding process.
[0011] One of the metals in the layered bimetallic oxide is calcium or magnesium, and the other metal is aluminum or iron; preferably, it is any one or more of layered calcium aluminum bimetallic oxide and layered magnesium aluminum bimetallic oxide.
[0012] In the S material, the weight parts of the raw materials are as follows: 18-25 parts of boron oxide; 25-35 parts of iron-barium slag; 40-50 parts of electric furnace phosphorus slag.
[0013] In order to save costs, the boron oxide can be industrial grade, with a main content of ≥99%. In the raw material calcination stage, boron oxide as a stabilizer can inhibit the crystal transformation of β-C2S to γ-C2S, which can prevent the strength of cement clinker from decreasing; in the cement hydration stage, boron oxide as a retarder can effectively regulate the cement setting time, prevent the activated components from accelerating cement hydration, and significantly shorten the cement setting time.
[0014] In the iron-barium slag, the mass percentage of barium oxide is not less than 20%, and the mass percentage of iron oxide is not more than 5%. During the raw material calcination stage, the glassy barium oxide can, on the one hand, promote the crystal transformation of β-C2S to generate more active α-C2S, stimulate the early strength of C2S, and on the other hand, can stabilize the high-temperature crystal phase with a trace amount of iron oxide, hinder the transformation of C3S to C2S, reduce the calcination temperature, and improve the calcinability of the raw material.
[0015] The phosphorus oxide content in the electric furnace phosphorus slag is 2.5% to 5.0% by mass. In the raw material calcination stage, trace phosphorus elements can reduce the solid phase reaction activation energy, increase the liquid phase volume, reduce the sintering temperature, and improve the raw material sinterability.
[0016] In the L material, the weight parts of each raw material are as follows: 10-15 parts of polymer polyol solution; 20-25 parts of ultrafine layered bimetallic oxide; 35-40 parts of industrial by-product sodium thiocyanate solution; and 20-35 parts of water.
[0017] The mass concentration of the polymerized polyol solution is 85-90%; the polymerized polyol is composed of polyols and polyglycerol esters, wherein the polyols are any two or three of glycerol, diglycerol and trimerol; the polymerized polyol contains a large number of polar hydroxyl groups, has extremely strong dispersibility and antistatic effects, increases the fluidity of materials, effectively improves the grinding efficiency of cement particles, and can reduce the power consumption of grinding while increasing the output of cement mills; in terms of physics, the mechanical strength of cement can be improved by improving the fineness of cement particles and optimizing the grading of cement particles; in terms of chemistry, certain components in the polymerized polyol can react chemically with metal oxides in cement, increase the activity of cement by causing lattice defects, and effectively improve the mechanical strength of cement;
[0018] The mass percentage of sodium thiocyanate in the industrial byproduct sodium thiocyanate solution is 45% to 50%. The introduction of sodium thiocyanate can increase the early hydration heat release rate and heat release of cement, improve the hydration degree of cement, increase the number of hydration products of the slurry, reduce the porosity, and reduce the pore size, which is beneficial to the development of early strength of cement.
[0019] The layered bimetallic oxide is made by coprecipitation method, and the specific surface area is controlled at 100m after ball milling. 2 / g~150m 2 / g range. Due to its high specific surface area, layered bimetallic oxides can play a micro-aggregate filling effect and nucleation effect in the cement hydration stage, provide nuclei for the hydration and crystallization of C3S and C2S, improve the degree of cement hydration, reduce porosity, and promote the development of cement 3d and 28d strength. At the same time, layered bimetallic oxides have the ability to efficiently capture CO2, which can significantly improve the anti-carbonization performance of cement-based materials.
[0020] The preparation method of the S material in the cement activator provided by the present invention is: respectively subjecting iron-barium slag and electric furnace phosphorus slag to ball milling, drying and screening to obtain iron-barium slag powder and electric furnace phosphorus slag powder, and uniformly mixing the two with boron oxide; the preparation method of the L material is: after mixing an industrial by-product sodium thiocyanate solution and water, adding the ball-milled layered bimetallic oxide, and obtaining a uniformly dispersed suspension after high-speed shear stirring, and then adding a polymerized polyol to the suspension, and stirring and mixing.
[0021] Furthermore, the ball milling conditions are: using a planetary ball mill, the ball mill speed is in the range of 400r / min to 500r / min, and the ball milling time is in the range of 60min to 90min.
[0022] The drying conditions are as follows: the drying temperature is between 100° C. and 105° C., and the material is dried until it has a constant weight.
[0023] The screening condition is: the test sieve mesh number is 200 meshes.
[0024] The conditions for high-speed shearing are: a stirring speed in the range of 3000 r / min to 5000 r / min, and a stirring time in the range of 60 min to 90 min.
[0025] The invention also provides a method for using the cement activator. The S material in the cement activator is used in the raw material grinding process, and the L material is used in the cement grinding process.
[0026] Furthermore, the S material in the cement activator is ground together with the raw meal, and the addition amount is 2% to 5% of the total mass of the raw meal.
[0027] The L material in the cement activator is ground together with cement clinker, gypsum and mixed materials, and the addition amount is 0.05% to 0.2% of the total mass of cement.
[0028] The present invention also provides the use of the cement activator as a cement admixture, and the S material and the L material in the cement activator are used as raw materials and cement admixtures respectively.
[0029] The cement activator provided by the present invention is composed of S material and L material. The S material is used in the raw material calcination stage, can regulate the crystal transformation of C2S, stimulate the early hydration activity of α-C2S, promote the early strength development of cement, and introduce trace elements (barium, iron and phosphorus) to reduce the activation energy of solid phase reaction, increase the liquid phase amount, reduce the firing temperature, improve the burnability of raw materials, and reduce the coal consumption of firing. The L material is used in the cement grinding stage and cement hydration stage. During the cement grinding stage, on the one hand, it can optimize the cement particle grading and enhance the activity of cement particles, promote the joint growth of cement 3d and 28d strength, and on the other hand, it can improve the grinding efficiency of cement clinker, reduce grinding power consumption, and increase hourly output; during the cement hydration stage, the introduction of industrial by-product sodium thiocyanate can accelerate the reaction rate of cement hydration and increase the number of early hydration products of cement, while the layered bimetallic oxides can play a micro-aggregate filling effect and nucleation effect. The high specific surface area can provide a large number of crystal nuclei for the hydration and crystallization of C3S and C2S, further improve the degree of cement hydration, reduce porosity, and promote the development of cement 3d and 28d strength.
[0030] S material and L material have complementary effects. In terms of reinforcement, S material acts on raw materials and improves the early strength of clinker by regulating the crystal transformation. L material acts on cement, mainly to improve the late strength of cement, and also improves the early strength of cement to a certain extent. In terms of energy saving, S material can reduce the clinker standard coal consumption during the calcination of raw materials, and L material can reduce the power consumption of cement grinding. At the same time, since S material and L material have a reinforcing effect on cement in both the early and late stages, they can also save energy and reduce emissions by reducing the clinker mix ratio.
[0031] Compared with the prior art, the present invention has the following advantages:
[0032] 1. The present invention combines the characteristics of the material itself to develop a dual-material cement activator, which stimulates the mechanical strength of cement from multiple stages of raw material calcination-cement grinding-cement hydration. It can promote the joint growth of cement 3d and 28d strength under the premise of reducing the cement clinker mix ratio, and reduce CO2 emissions by replacing clinker.
[0033] 2. During the raw material calcination stage, the trace elements in the S material can improve the burnability of the raw material and reduce the coal consumption during burning; during the cement grinding stage, the polymer polyols in the L material can improve the grinding efficiency of cement particles, increase the output of the cement mill and reduce the power consumption of grinding. Under the combined effect of the two, the energy consumption of cement production can be effectively reduced, and CO2 emissions can be further reduced.
[0034] 3. The layered bimetallic oxides used in the L material have a high specific surface area, which can provide a large number of crystal nuclei for the hydration and crystallization of C3S and C2S, improve the degree of cement hydration, promote the formation of cement products, reduce porosity, and help improve the mechanical strength of cement at 3d and 28d hydration ages; at the same time, it has the ability to efficiently capture CO2, which can significantly improve the anti-carbonation performance of cement-based materials.
[0035] 4. The present invention is based on the basic principle of green development and realizes the resource utilization of industrial wastes such as iron-barium slag, electric furnace phosphorus slag and industrial by-product sodium thiocyanate solution. The developed high-efficiency and energy-saving cement activator does not introduce any toxic or polluting raw materials, is green, safe and environmentally friendly, has no chlorine or alcohol amine components, has low production cost and is easy to use. DETAILED DESCRIPTION
[0036] The layered calcium aluminum bimetallic oxide and the layered magnesium aluminum bimetallic oxide in each embodiment and comparative example are prepared according to the method in the following literature: Li Xiaoyan, Liu Yibao, Zhang Weimin, et al., Study on the performance of layered bimetallic oxide adsorbing boron in solution, Functional Materials, Vol. (48), 2017, 02020-02025. It can also be prepared according to the method disclosed in other literature. The specific preparation process is as follows:
[0037] Layered calcium aluminum bimetallic oxide: Add 1200 mL of water to the reactor, weigh 92.4 g of calcium nitrate hexahydrate and 45.0 g of aluminum nitrate nonahydrate, slowly add them to the reactor, and stir at a speed of 150 r / min until they are evenly mixed; add 2.5 mol / L sodium hydroxide solution dropwise to the reactor, control the pH value of the reaction solution between 9 and 11, and carry out the reaction process under nitrogen protection. The precipitation reaction time is 2 h; filter the milky white slurry, and heat it in a water bath. The aging process is carried out by controlling the water bath heating temperature to 70°C and the aging time to 18h to form a colloidal precipitate. The colloidal precipitate is placed in a 105°C forced air drying oven for drying. After drying, it is placed in a muffle furnace for high-temperature calcination. The calcination temperature is controlled to be 520°C and the calcination time is 6h. After cooling to room temperature, it is fully ground. The ball mill speed is 800r / min and the ball milling time is 120min. An ultrafine layered calcium aluminum bimetallic oxide with a specific surface area in the range of 100m2 / g to 150m2 / g can be prepared.
[0038] Layered magnesium aluminum bimetallic oxide: add 1200 mL of water to the reactor, weigh 92.4 g of magnesium nitrate hexahydrate and 45.0 g of hydrated aluminum nitrate in turn, slowly add them to the reactor in turn, and stir at a speed of 200 r / min until they are evenly mixed; add 3.5 mol / L sodium hydroxide solution dropwise to the reactor, control the pH value of the reaction solution between 9 and 11, and carry out the reaction process under nitrogen protection. The precipitation reaction time is 2.5 h; filter the milky white slurry, and heat it in a water bath Aging is carried out, the water bath heating temperature is controlled at 90°C, the aging time is 12h, and a colloidal precipitate is formed; the colloidal precipitate is placed in a 100°C forced air drying oven for drying, and after drying, it is placed in a muffle furnace for high-temperature roasting, the roasting temperature is controlled at 570°C, the roasting time is 4h, and after cooling to room temperature, it is fully ground, the ball mill speed is 900r / min, and the ball milling time is 90min, and an ultrafine layered magnesium-aluminum bimetallic oxide with a specific surface area in the range of 100m2 / g to 150m2 / g can be prepared.
[0039] The iron-barium slag is purchased from Shandong Zhongcheng Barium Salt Chemical Co., Ltd., and its barium oxide mass percentage is not less than 20%, and its iron oxide mass percentage is not more than 5%.
[0040] The electric furnace phosphorus slag was purchased from Maanshan Iron and Steel Co., Ltd., and the mass percentage of phosphorus oxide was 2.5% to 5.0%.
[0041] The polymeric polyol solution was purchased from Shandong Taixi Chemical Co., Ltd., and its mass concentration was 85-90%.
[0042] The industrial by-product sodium thiocyanate solution was purchased from Jinan Jingyu New Material Technology Co., Ltd., in which the mass percentage of sodium thiocyanate was 45% to 50%.
[0043] Unless otherwise specified, the test materials and reagents used in the examples can be obtained from commercial sources.
[0044] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0045] The present invention is described in detail below with reference to the embodiments.
[0046] Example 1
[0047] A high-efficiency energy-saving cement activator is composed of S material and L material. The weight parts of the components in the S material are: 25 parts of boron oxide; 25 parts of iron-barium slag; 50 parts of electric furnace phosphorus slag; the weight parts of the components in the L material are: 10 parts of polymerized polyol solution; 25 parts of ultrafine layered calcium aluminum bimetallic oxide; 35 parts of industrial by-product sodium thiocyanate solution; and 30 parts of water.
[0048] The preparation method of the S material in the above-mentioned high-efficiency energy-saving cement activator comprises the following steps:
[0049] 1) Weigh 500g of iron-barium slag, and perform ball milling, drying and screening in sequence, wherein the ball milling parameters include: the ball mill speed is 400r / min, and the ball milling time is 90min. The iron-barium slag after ball milling is placed in a drying oven at 100°C and dried to a constant weight state, and sieved through a 200-mesh test sieve to obtain barium slag powder;
[0050] 2) Weigh 1000g of electric furnace phosphorus slag, and perform ball milling, drying and screening in sequence, wherein the ball milling parameters include: the ball mill speed is 400r / min, and the ball milling time is 90min. The ball-milled electric furnace slag is placed in a drying oven at 100°C and dried to a constant weight state, and sieved through a 200-mesh test sieve to obtain phosphorus slag powder;
[0051] 3) Boron oxide, barium slag powder and phosphorus slag powder were weighed in sequence according to the formula, and mixed evenly with a mixer at a mixer speed of 200 r / min for a mixing time of 150 min to obtain S material.
[0052] The preparation method of the L material in the above-mentioned high-efficiency energy-saving cement activator comprises the following steps:
[0053] 1) After mixing the formulated amount of industrial byproduct sodium thiocyanate solution and water, add ultrafine layered calcium aluminum bimetallic oxide, and stir at a high speed of 3000 r / min for 90 minutes to obtain a uniformly dispersed suspension;
[0054] 2) Add the polymer polyol solution to the suspension and stir at a speed of 200 r / min for 60 min to obtain material L.
[0055] In the above-mentioned high-efficiency energy-saving cement activator, the content of S material in the raw meal is 2%, and the content of L material in the cement is 0.2%.
[0056] Example 2
[0057] A high-efficiency energy-saving cement activator is composed of S material and L material. The weight parts of the components in the S material are: 25 parts of boron oxide; 25 parts of iron-barium slag; 50 parts of electric furnace phosphorus slag; the weight parts of the components in the L material are: 15 parts of polymerized polyol solution; 20 parts of ultrafine layered calcium aluminum bimetallic oxide; 40 parts of industrial by-product sodium thiocyanate solution; and 25 parts of water.
[0058] The preparation method of the S material in the above-mentioned high-efficiency energy-saving cement activator comprises the following steps:
[0059] 1) Weigh 500g of iron-barium slag, and perform ball milling, drying and screening in sequence, wherein the ball milling parameters include: the ball mill speed is 400r / min, and the ball milling time is 90min. The iron-barium slag after ball milling is placed in a drying oven at 100°C and dried to a constant weight state, and sieved through a 200-mesh test sieve to obtain barium slag powder;
[0060] 2) Weigh 1000g of electric furnace phosphorus slag, and perform ball milling, drying and screening in sequence, wherein the ball milling parameters include: the ball mill speed is 400r / min, and the ball milling time is 90min. The ball-milled electric furnace phosphorus slag is placed in a drying oven at 100°C and dried to a constant weight state, and sieved through a 200-mesh test sieve to obtain phosphorus slag powder;
[0061] 3) Boron oxide, barium slag powder and phosphorus slag powder were weighed in sequence according to the formula, and mixed evenly with a mixer at a mixer speed of 200 r / min for a mixing time of 150 min to obtain S material.
[0062] The preparation method of the L material in the above-mentioned high-efficiency energy-saving cement activator comprises the following steps:
[0063] 1) After mixing the formulated amount of industrial byproduct sodium thiocyanate solution and water, add ultrafine layered calcium aluminum bimetallic oxide, and high-speed shear stirring at a speed of 5000r / min for 60min to obtain a uniformly dispersed suspension;
[0064] 2) Add the polymer polyol solution to the suspension and stir at a speed of 300 r / min for 30 min to obtain material L.
[0065] In the above-mentioned high-efficiency energy-saving cement activator, the content of S material in the raw meal is 5%, and the content of L material in the cement is 0.05%.
[0066] Example 3
[0067] A high-efficiency energy-saving cement activator is composed of S material and L material. The weight parts of the components in the S material are: 18 parts of boron oxide; 35 parts of iron-barium slag; 47 parts of electric furnace phosphorus slag; the weight parts of the components in the L material are: 10 parts of polymer polyol solution; 25 parts of ultrafine layered magnesium-aluminum bimetallic oxide; 35 parts of industrial by-product sodium thiocyanate solution; and 30 parts of water.
[0068] The preparation method of the S material in the above-mentioned high-efficiency energy-saving cement activator comprises the following steps:
[0069] 1) Weigh 500g of iron-containing barium slag, and perform ball milling, drying and screening in sequence, wherein the ball milling parameters include: the ball mill speed is 500r / min, and the ball milling time is 60min. The iron-containing barium slag after ball milling is placed in a drying oven at 105°C and dried to a constant weight state, and sieved through a 200-mesh test sieve to obtain barium slag powder;
[0070] 2) Weigh 1000g of electric furnace phosphorus slag, and perform ball milling, drying and screening in sequence, wherein the ball milling parameters include: the ball mill speed is 500r / min, and the ball milling time is 60min. The ball-milled electric furnace slag is placed in a drying oven at 105°C and dried to a constant weight state, and sieved through a 200-mesh test sieve to obtain phosphorus slag powder;
[0071] 3) Boron oxide, barium slag powder and phosphorus slag powder were weighed in sequence according to the formula, and mixed evenly with a mixer at a mixer speed of 300 r / min for a mixing time of 120 min to obtain S material.
[0072] The preparation method of the L material in the above-mentioned high-efficiency energy-saving cement activator comprises the following steps:
[0073] 1) After mixing the formulated amount of industrial byproduct sodium thiocyanate solution and water, adding ultrafine layered magnesium aluminum bimetallic oxide, and high-speed shear stirring at a speed of 3000r / min for 90min to obtain a uniformly dispersed suspension;
[0074] 2) Add the polymer polyol solution to the suspension and stir at a speed of 200 r / min for 60 min to obtain material L.
[0075] In the above-mentioned high-efficiency energy-saving cement activator, the content of S material in the raw meal is 4%, and the content of L material in the cement is 0.1%.
[0076] Example 4
[0077] A high-efficiency energy-saving cement activator is composed of S material and L material. The weight parts of the components of the S material are: 18 parts of boron oxide; 35 parts of iron-barium slag; 47 parts of electric furnace phosphorus slag; the weight parts of the components of the L material are: 15 parts of polymerized polyol solution; 20 parts of ultrafine layered magnesium-aluminum bimetallic oxide; 40 parts of industrial by-product sodium thiocyanate solution; and 25 parts of water.
[0078] The preparation method of the S material in the above-mentioned high-efficiency energy-saving cement activator comprises the following steps:
[0079] 1) Weigh 500g of iron-containing barium slag, and perform ball milling, drying and screening in sequence, wherein the ball milling parameters include: the ball mill speed is 500r / min, and the ball milling time is 60min. The iron-containing barium slag after ball milling is placed in a drying oven at 105°C and dried to a constant weight state, and sieved through a 200-mesh test sieve to obtain barium slag powder;
[0080] 2) Weigh 1000g of electric furnace phosphorus slag, and perform ball milling, drying and screening in sequence, wherein the ball milling parameters include: the ball mill speed is 500r / min, and the ball milling time is 60min. The ball-milled electric furnace slag is placed in a drying oven at 105°C and dried to a constant weight state, and sieved through a 200-mesh test sieve to obtain phosphorus slag powder;
[0081] 3) Boron oxide, barium slag powder and phosphorus slag powder were weighed in sequence according to the formula, and mixed evenly with a mixer at a mixer speed of 300 r / min for a mixing time of 120 min to obtain S material.
[0082] The preparation method of the L material in the above-mentioned high-efficiency energy-saving cement activator comprises the following steps:
[0083] 1) After mixing the formulated amount of industrial byproduct sodium thiocyanate solution and water, adding ultrafine layered magnesium aluminum bimetallic oxide, and high-speed shear stirring at a speed of 5000r / min for 60min to obtain a uniformly dispersed suspension;
[0084] 2) Add the polymer polyol solution to the suspension and stir at a speed of 300 r / min for 30 min to obtain material L.
[0085] In the above-mentioned high-efficiency energy-saving cement activator, the content of S material in the raw meal is 3%, and the content of L material in the cement is 0.1%.
[0086] Comparative Example 1
[0087] The only difference between Comparative Example 1 and Example 1 is that no L material is added in Comparative Example 1, and the components and contents of S material are consistent with those in Example 1.
[0088] That is, the high-efficiency energy-saving cement activator provided in Comparative Example 1 is composed only of S material, and the mass percentages of the components of the S material are: 25 parts of boron oxide; 25 parts of iron-barium slag; and 50 parts of electric furnace phosphorus slag.
[0089] The preparation method of material S in the high-efficiency and energy-saving cement activator of comparative example 1 is consistent with that of example 1.
[0090] The dosage of S material in the high-efficiency energy-saving cement activator of Comparative Example 1 is consistent with that of Example 1.
[0091] Comparative Example 2
[0092] The only difference between Comparative Example 2 and Example 1 is that no S material is added in Comparative Example 2, and the components and contents of L material are consistent with those in Example 1.
[0093] That is, the high-efficiency and energy-saving cement activator provided in Comparative Example 2 is composed only of L material, and the mass percentages of the components of L material are: 10 parts of polymer polyol solution; 25 parts of ultrafine layered calcium aluminum bimetallic oxide; 35 parts of industrial by-product sodium thiocyanate solution; and 30 parts of water.
[0094] The preparation method of material L in the high-efficiency and energy-saving cement activator of comparative example 2 is consistent with that of example 1.
[0095] The dosage of L material in the high-efficiency energy-saving cement activator of Comparative Example 2 is consistent with that of Example 1.
[0096] Comparative Example 3
[0097] The only difference between Comparative Example 3 and Example 2 is that no iron-barium slag is added to the S material of Comparative Example 3, and the other components and their contents are consistent with those of Example 2.
[0098] That is, the high-efficiency and energy-saving cement activator provided in Comparative Example 2, the mass percentages of the components of the S material are: 25 parts of boron oxide; 50 parts of electric furnace phosphorus slag; the mass percentages of the components of the L material are: 15 parts of polymer polyol solution; 20 parts of ultrafine layered calcium aluminum bimetallic oxide; 40 parts of industrial by-product sodium thiocyanate solution; 25 parts of water.
[0099] Comparative Example 3 The preparation method of S material in the high-efficiency energy-saving cement activator is compared with Example 2, except that only the barium slag powder in step 1) and step 3) is deleted;
[0100] The preparation method of material L in the high-efficiency energy-saving cement activator in Comparative Example 3 is consistent with that in Example 2.
[0101] The dosage of S material and L material in the high-efficiency energy-saving cement activator of Comparative Example 3 is consistent with that of Example 2.
[0102] Comparative Example 4
[0103] The only difference between Comparative Example 4 and Example 2 is that no electric furnace phosphorus slag is added to the S material of Comparative Example 4, and the other components and their contents are consistent with those of Example 2.
[0104] That is, the high-efficiency and energy-saving cement activator provided in Comparative Example 4, the mass percentages of the components of the S material are: 25 parts of boron oxide; 25 parts of iron-barium slag; the mass percentages of the components of the L material are: 15 parts of polymer polyol solution; 20 parts of ultrafine layered calcium aluminum bimetallic oxide; 40 parts of industrial by-product sodium thiocyanate solution; 25 parts of water.
[0105] Comparative Example 4 The preparation method of S material in the high-efficiency energy-saving cement activator is compared with Example 2, except that only the phosphorus slag powder in step 2) and step 3) is deleted;
[0106] The preparation method of material L in the high-efficiency energy-saving cement activator in Comparative Example 4 is consistent with that in Example 2.
[0107] The dosage of S material and L material in the high-efficiency energy-saving cement activator of Comparative Example 4 is consistent with that of Example 2.
[0108] Comparative Example 5
[0109] The only difference between Comparative Example 5 and Example 3 is that no boron oxide is added to the S material of Comparative Example 5, and the other components and their contents are consistent with those of Example 3.
[0110] That is, in the high-efficiency energy-saving cement activator provided in Comparative Example 5, the mass percentages of the components of the S material are: 35 parts of iron-barium slag; 47 parts of electric furnace phosphorus slag; the mass percentages of the components of the L material are: 10 parts of polymer polyol solution; 25 parts of ultrafine layered magnesium aluminum bimetallic oxide; 35 parts of industrial by-product sodium thiocyanate solution; and 30 parts of water.
[0111] The preparation method of material S in the energy-efficient cement activator of comparative example 5 is compared with that of example 3, except that only the boron oxide in step 3) is deleted;
[0112] The preparation method of material L in the high-efficiency energy-saving cement activator in Comparative Example 5 is consistent with that in Example 3.
[0113] The dosage of S material and L material in the high-efficiency energy-saving cement activator of Comparative Example 5 is consistent with that of Example 3.
[0114] Comparative Example 6
[0115] The only difference between Comparative Example 6 and Example 3 is that no polymer polyol solution is added to the L material of Comparative Example 6, and the remaining components and their contents are consistent with those of Example 3.
[0116] That is, in the high-efficiency and energy-saving cement activator provided in Comparative Example 6, the mass percentages of the components of the S material are: 18 parts of boron oxide; 35 parts of iron-barium slag; 47 parts of electric furnace phosphorus slag; the mass percentages of the components of the L material are: 25 parts of ultrafine layered magnesium-aluminum bimetallic oxide; 35 parts of industrial by-product sodium thiocyanate solution; and 30 parts of water.
[0117] The preparation method of material S in the high-efficiency energy-saving cement activator of comparative example 6 is consistent with that of example 3;
[0118] The preparation method of the L material in the high-efficiency energy-saving cement activator in Comparative Example 6 is compared with that in Example 3, except that only step 3) is deleted.
[0119] The dosage of S material and L material in the high-efficiency energy-saving cement activator of Comparative Example 6 is consistent with that of Example 3.
[0120] Comparative Example 7
[0121] The only difference between Comparative Example 7 and Example 4 is that no ultrafine layered magnesium-aluminum bimetallic oxide is added to the L material of Comparative Example 7, and the remaining components and their contents are consistent with those of Example 4.
[0122] That is, the high-efficiency and energy-saving cement activator provided in Comparative Example 7, the mass percentages of the components of S material are: 18 parts of boron oxide; 35 parts of iron-barium slag; 47 parts of electric furnace phosphorus slag; the mass percentages of the components of L material are: 15 parts of polymer polyol solution; 40 parts of industrial by-product sodium thiocyanate solution; 25 parts of water.
[0123] The preparation method of the S material in the high-efficiency energy-saving cement activator of Comparative Example 7 is consistent with that of Example 4;
[0124] Compared with Example 4, the preparation method of material L in the high-efficiency energy-saving cement activator in Comparative Example 7 deletes the ultrafine layered bimetallic oxide in step 1) and step 2).
[0125] The dosage of S material and L material in the high-efficiency energy-saving cement activator of Comparative Example 7 is consistent with that of Example 4.
[0126] Comparative Example 8
[0127] The only difference between Comparative Example 8 and Example 4 is that no industrial by-product sodium thiocyanate solution is added to the L material of Comparative Example 8, and the remaining components and their contents are consistent with those of Example 4.
[0128] That is, in the high-efficiency energy-saving cement activator provided in Comparative Example 8, the mass percentages of the components of the S material are: 18 parts of boron oxide; 35 parts of iron-barium slag; 47 parts of electric furnace phosphorus slag; the mass percentages of the components of the L material are: 15 parts of polymerized polyol solution; 20 parts of ultrafine layered magnesium-aluminum bimetallic oxide; and 25 parts of water.
[0129] The preparation method of the S material in the high-efficiency energy-saving cement activator of Comparative Example 8 is consistent with that of Example 4;
[0130] The preparation method of material L in the high-efficiency energy-saving cement activator in Comparative Example 8 is compared with that in Example 4, except that the industrial by-product sodium thiocyanate solution in step 2) is deleted.
[0131] The dosage of S material and L material in the high-efficiency energy-saving cement activator of Comparative Example 8 is consistent with that of Example 4.
[0132] The S material and L material in the cement activator prepared in the above embodiments and comparative examples are added in the raw material grinding process and cement grinding process according to their respective specified dosages. The mass percentage of each raw material in cement is: clinker 74%, desulfurized gypsum 5%, limestone powder 5%, fly ash 10%, and volcanic ash 6%.
[0133] A control group 1 and a control group 2 are set, and the raw materials and cement in the control group 1 and the control group 2 are not ground with the addition of an activator, and the types of raw materials and clinkers are the same as those in the embodiments and comparative examples. The weight percentages of the raw materials in the cement in the control group 1 are: 78% clinker, 5% desulfurized gypsum, 5% limestone powder, 6% fly ash, and 6% volcanic ash; the weight percentages of the raw materials in the cement in the control group 2 are: 74% clinker, 5% desulfurized gypsum, 5% limestone powder, 10% fly ash, and 6% volcanic ash.
[0134] In accordance with the provisions of GB175-2023 "General Portland Cement", the method specified in GB / T 17671-1999 "Test Method for Cement Mortar Strength" was adopted, cement, standard sand and water were mixed in a ratio of 1:3.0:0.5, and standard test pieces of 40mm×40mm×160mm were made. The test pieces were cured under standard curing conditions, and their compressive strengths at 3d and 28d were measured respectively.
[0135] The cement sieve residue was tested according to GB / T 1345-2005 “Cement fineness test method - sieve analysis method”; the cement specific surface area was tested using the Blaine method. The test results are shown in the following table.
[0136]
[0137]
[0138] According to the statistical results of the performance tests of the control group and the embodiments, when 4% fly ash is used to replace clinker, the compressive strength of the cement added with the activator at the hydration age of 3d and 28d is increased, the standard coal consumption of clinker and the power consumption of cement grinding are significantly reduced, the cement residue is relatively reduced, and the specific surface area is relatively increased. This shows that the cement activator provided by the present invention has many functions such as strengthening, energy saving and emission reduction, and optimization of particle grading.
[0139] According to the statistical results of the performance tests of Example 1 and Comparative Example 1, when L material is added, the activator will cause the cement residue to be relatively reduced and the specific surface area to be relatively increased. At the same time, it can effectively reduce the power consumption of cement grinding and promote the further development of the early strength of cement.
[0140] According to the statistical results of the performance tests of Example 1 and Comparative Example 2, when S material is added, the activator will significantly reduce the standard coal consumption of clinker, and at the same time it is beneficial to promote the improvement of the 3d compressive strength of cement.
[0141] According to the performance test statistical results of Example 2 and Comparative Example 3, when iron-barium slag is added to the S material, the standard coal consumption of clinker is relatively reduced, and the 3d compressive strength of cement is significantly increased.
[0142] According to the statistical results of the performance tests of Example 2 and Comparative Example 4, when electric furnace phosphorus slag is added to the S material, the standard coal consumption of clinker is significantly reduced, while other index parameters fluctuate slightly.
[0143] According to the statistical results of the performance tests of Example 3 and Comparative Example 5, when boron oxide is added to the S material, the crystal transformation of C2S is promoted, which is beneficial to the early strength development of cement.
[0144] According to the statistical results of the performance tests of Example 3 and Comparative Example 6, when polymerized polyols are added to the L material, the cement residue is relatively reduced, the specific surface area is significantly increased, and the power consumption of cement grinding is also reduced.
[0145] According to the statistical results of the performance tests of Example 4 and Comparative Example 7, when ultrafine layered bimetallic oxides are added to the L material, the compressive strength of the cement at the hydration age of 3d and 28d is improved.
[0146] According to the performance test statistical results of Example 4 and Comparative Example 8, when the industrial by-product sodium thiocyanate solution is added to the L material, the 3d compressive strength of the cement can be increased.
[0147] The detailed description of a high-efficiency and energy-saving cement activator and a preparation method thereof with reference to the above-mentioned embodiments is illustrative rather than restrictive, and several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.
Claims
1. A cement activator, characterized in that: The cement activator consists of S material and L material. The S material includes boron oxide, iron-barium slag and electric furnace phosphorus slag; the L material includes polymer polyol solution, layered bimetallic oxide, industrial byproduct sodium thiocyanate solution and water.
2. The cement activator according to claim 1, characterized in that The S material is used in the raw material grinding process; the L material is used in the cement grinding process.
3. The cement activator according to claim 1, characterized in that One of the metals in the layered bimetallic oxide is calcium or magnesium, and the other metal is aluminum or iron.
4. The cement activator according to any one of claims 1 to 3, characterized in that: In the S material, the weight parts of the raw materials are as follows: 18-25 parts of boron oxide; 25-35 parts of iron-barium slag; 40-50 parts of electric furnace phosphorus slag.
5. The cement activator according to claim 4, characterized in that In the iron-barium slag, the mass percentage of barium oxide is not less than 20%, and the mass percentage of iron oxide is not more than 5%; in the electric furnace phosphorus slag, the mass percentage of phosphorus oxide is 2.5% to 5.0%.
6. The cement activator according to any one of claims 1 to 3, characterized in that: In the L material, the weight parts of each raw material are as follows: 10-15 parts of polymer polyol solution; 20-25 parts of ultrafine layered bimetallic oxide; 35-40 parts of industrial by-product sodium thiocyanate solution; and 20-35 parts of water.
7. The cement activator according to claim 6, characterized in that The mass concentration of the polymer polyol solution is 85-90%; the mass percentage of sodium thiocyanate in the industrial byproduct sodium thiocyanate solution is 45-50%.
8. The method for preparing a cement activator according to any one of claims 1 to 7, characterized in that: The preparation method of the S material in the cement activator is: respectively subjecting iron-barium slag and electric furnace phosphorus slag to ball milling, drying and screening to obtain iron-barium slag powder and electric furnace phosphorus slag powder, and uniformly mixing the two with boron oxide; the preparation method of the L material is: after mixing the industrial by-product sodium thiocyanate solution and water, adding the ball-milled layered bimetallic oxide, after high-speed shear stirring, obtaining a uniformly dispersed suspension, and then adding polymerized polyol to the suspension, stirring and mixing.
9. The method for using the cement activator according to any one of claims 1 to 7, characterized in that: The S material in the cement activator is used in the raw material grinding process, and the L material is used in the cement clinker grinding process.
10. Use of the cement activator according to any one of claims 1 to 7 as a cement admixture.
Citation Information
Patent Citations
Environment-friendly high-strength cement and preparation method thereof
CN111187013A
Chlorine-free cement grinding aid and preparation method thereof
CN111689714A
Pervious concrete capable of efficiently adsorbing carbon dioxide through cooperation of multiple solid wastes and preparation method of pervious concrete
CN116283141A
Preparation method and application method of efficient chloride ion curing agent for sea sand mortar
CN116891358A
KZ22910A4