Wall protection slurry suitable for river-facing geology and construction method
By developing suitable wall-protecting mud ratio and construction methods under riverside geological conditions, the problems of hole collapse and slurry leakage caused by poor mud ratio are solved, and the stability of slot holes and construction efficiency are improved.
Patent Information
- Application Number
- CN202411133626.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-12
AI Technical Summary
Under riverside geological conditions, poor mud ratio leads to problems such as hole collapse, neck shrinkage, and slurry leakage often occur during trough formation and hole formation, affecting the quality and efficiency of the project.
A wall protection mud suitable for riverside geology has been developed, containing bentonite, soda ash, hydroxypropyl methylcellulose, thickener and cement. Through specific proportions and construction methods, high density, good rheology and toughness are formed. Strong mud, injected into the slot holes to keep the hole wall stable and avoid collapse and leakage of slurry.
It effectively avoids the collapse of holes and necking in the trough, improves the quality of the trough, reduces waste of concrete materials, reduces engineering costs, and improves the bearing capacity of the seepage intercept wall and cast-injected piles.
Smart Images

Figure CN118930149A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building construction, and in particular relates to a wall protection slurry suitable for riverside geology and a construction method. Background Art
[0002] Mud wall protection is the most widely used trenching and hole-forming method for underground continuous wall and cast-in-place pile construction. The quality of mud is the key to high-quality trenching and hole-forming construction. The mud ratio often needs to be configured according to different construction environments. If the mud ratio is not good and cannot adapt to the construction soil layer, it is very easy to collapse the hole during the trenching and hole-forming process, affecting the quality of the project. Especially for some soft soil layers, if the mud ratio of general soil layers is copied, problems such as wall and pile shrinkage, broken piles, and mud leakage are likely to occur.
[0003] The shallow foundation soil of Linjiang Geology is mainly silty silty loam, with low shear strength and extremely soft soil. The liquid index is 0.95-1.78, which is in a plastic state. Its permeability coefficient is 10 -6 cm / s, which is a relatively impermeable layer; the lower part of the stratum is mostly silt and fine sand layers, the soil is loose, and its permeability coefficient is 10 -2 cm / s, strong water permeability. The groundwater of the proposed site is divided into groundwater and confined water. The groundwater level is relatively high, mainly supplied by atmospheric precipitation and surface water. The confined water with a lower water level is replenished with the water of the Yangtze River. The confined water head is high, which keeps the groundwater level elevation of the site at a relatively high level, resulting in a high moisture content of the upper silty silty loam. The slot holes are prone to shrinkage and collapse during the upper trenching construction. The lower silty sand layer is located in the water body. Under the action of confined water, quicksand is very likely to occur, resulting in hole collapse and even pipe bursts, and the conditions for trenching and hole formation are extremely poor.
[0004] Due to the quality problems of the cut-off wall construction, the foundation pit leakage of the riverside project is common, which not only restricts the progress of the project construction and requires measures to be taken to deal with it separately, but also affects the project benefits. The reasons for these are mostly related to the quality of trenching during the construction of the cut-off wall; at the same time, due to the low quality of the mud itself, the mud in the hole is diluted during the hole cleaning process, causing the mud specific gravity in the hole to decrease, resulting in hole collapse during the hole cleaning process. Once the steel cage is buried by the collapsed hole soil, it is difficult to deal with it and can only be re-constructed by filling the hole; and the poor quality of hole cleaning causes thick mud and sand deposition at the bottom of the hole and the bottom of the trench, seriously affecting the bearing capacity of the cut-off wall and the bored piles; and due to the common hole collapse phenomenon in the construction process of the cut-off wall trenching and bored pile drilling, the concrete pouring filling coefficient is generally between 1.2-1.25, which wastes concrete materials and increases the project cost.
[0005] In order to improve the construction quality of underground continuous walls and bored piles, a research method for wall protection slurry was proposed. According to the actual geological conditions on site, a slurry was developed. The slurry has high wall protection specific gravity, good rheological properties and strong toughness. It is suitable for the construction of cut-off walls and bored piles in riverside geology or similar geological conditions. It is suitable for soft strata with abundant groundwater, large seepage volume, and mainly composed of silty silty loam and fine sand layers. It can maintain the stability of the hole wall during the trenching process, effectively improve the trenching quality, and avoid problems such as diameter shrinkage, hole wall collapse and excessive sediment at the bottom of the trench during trenching construction. Summary of the invention
[0006] In view of this, the present invention aims to propose a wall protection mud and construction method suitable for riverside geology, so as to solve the problem that the mud ratio is poor, cannot adapt to soft soil layers, and is very easy to collapse during trenching and drilling, thus affecting the quality of the project.
[0007] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0008] The first aspect of the present invention provides a wall protection mud suitable for riverside geology, which comprises the following components by weight: 51-53kg of bentonite, 2.3-2.5kg of soda ash, 0.36-0.38kg of hydroxypropyl methylcellulose, 0.10-0.14kg of thickener, 0.06-0.08kg of cement, and 1000kg of water.
[0009] Furthermore, the following components are included by weight: 52 kg bentonite, 2.4 kg soda ash, 0.25 kg hydroxypropyl methylcellulose, 0.12 kg thickener, 0.07 kg cement, and 1000 kg water.
[0010] Furthermore, the bentonite is sodium-based bentonite; the thickener includes one or more of gypsum, ethoxylated sodium alkyl sulfide, and sodium dodecyl sulfonate.
[0011] The second aspect of the present invention provides a method for preparing a wall protection slurry suitable for riverside geology according to the first aspect of the present invention, comprising the following steps:
[0012] S1: Mix bentonite into water and stir evenly to obtain a mixed solution 1;
[0013] S2: mixing soda ash, hydroxypropyl methylcellulose, thickener and cement into water, stirring until fully hydrated, to obtain mixed solution 2;
[0014] S3: Mix the mixed solution 1 and the mixed solution 2 to obtain slurry.
[0015] The third aspect of the present invention provides a construction method of a wall protection slurry suitable for riverside geology according to the first aspect of the present invention, comprising the following steps:
[0016] S1: Measure and locate the pile position of the cut-off wall, drill holes at the pile position, take soil, and construct the guide groove;
[0017] S2: The trenching equipment drills a hole and injects the mud described in the first aspect of the present invention to remove drilling debris. The mud level is higher than the groundwater level by more than 1.0 m to maintain a high head difference inside and outside the trench;
[0018] S3: circulating the slurry;
[0019] S4: Take out the drilling equipment and install the steel cage and the guide tube in the slot;
[0020] S5: remove the sediment at the bottom of the slot;
[0021] S6: Detecting the mud in the slot.
[0022] Furthermore, the step S1 also includes leveling the construction site.
[0023] Furthermore, the guide groove in S1 includes a horizontal section and a vertical section. The horizontal section is arranged on the construction plane. The top surface of the horizontal section is 10 cm higher than the construction planes on both sides, and the distance between the top surface of the horizontal section and the mud liquid surface is 0.3-0.5 m to avoid overflow. The vertical section is arranged in the slot hole, and the inner diameter of the vertical section corresponds to the inner diameter of the slot hole.
[0024] Furthermore, before the injection of the mud in S2, the following steps are also included: the prepared mud is pumped into the mud pool for standby use, and the mud needs to be frequently stirred to keep the mud uniform and avoid sedimentation or segregation. The performance indicators of the mud in S1-S2 are: mud density 1.03-1.08g / cm 3 , funnel viscosity is 35-50s.
[0025] Furthermore, the specific step of S3 is: injecting mud into the slot hole, and using a mud pump to pump the mud containing suspended drilling cuttings in the slot hole from the drilling equipment into a waste mud pool for sedimentation treatment. During the slot construction process, due to the mixing of rock cuttings and the consumption of other treatment agents, the performance of the mud in the slot hole will gradually deteriorate, and a slurry replacement treatment is required.
[0026] Furthermore, the specific step of S5 is: injecting the mud that has been subjected to sedimentation treatment into the slot hole, and using a mud pump to pump the sediment at the bottom of the slot hole from the conduit into the waste slurry pool for sedimentation treatment.
[0027] Furthermore, in S6, the density of the mud in the slot is ≤1.15g / cm 3 , funnel viscosity is 32-50s, and sand content is ≤4%.
[0028] Furthermore, drainage ditches are set around the trough holes and the mud pool to prevent large amounts of surface sewage or rainwater from flowing in and contaminating the mud.
[0029] Furthermore, during trenching construction, additional stress on the trench wall caused by loads and equipment near the trench wall is avoided, and equipment vibration is reduced to avoid trench wall collapse due to external forces.
[0030] The fourth aspect of the present invention provides a quality control method for the wall protection slurry applicable to riverside geology as described in the first aspect of the present invention. The specific control method is as follows:
[0031] S1: The performance index of the mud just prepared in the mixer according to the first aspect of the present invention is tested, and the sampling time is 160-240 minutes after the mixer completes 3 Test once when the mud is being stirred;
[0032] S2: Testing the performance index of the mud stored in the mud pool, with sampling time once every 20-28 hours;
[0033] S3: The mud that has been purified by mud replacement needs to be tested for performance indicators before use. Samples are taken from the mud pool to test relevant indicators. If the mud density, funnel viscosity and sand content of the mud cannot meet the requirements, it is necessary to replace the mud with qualified ones.
[0034] S4: Testing the performance indexes of the mud in the tank, sampling and testing the upper mud in the tank when the tank is halfway deep and near the end.
[0035] Furthermore, the sampling time in S1 is when the mixer completes 200m 3 The mud is tested once when it is stirred; the sampling time in S2 is once every 24 hours.
[0036] Furthermore, the mud performance index in S1-S2 is: mud density 1.03-1.08g / cm 3 , funnel viscosity is 35-50s; the mud performance index in S3-S4 is: mud density ≤1.15g / cm 3 , funnel viscosity is 32-50s, and sand content is ≤4%.
[0037] The stability of the slot hole wall is related to the type of foundation, density and groundwater level. In actual construction, if the soil layer is loose, the hole wall will collapse inward under the horizontal pressure of the surrounding soil. Mud wall protection is an important way to ensure the stability of the slot hole. By injecting mud into the slot hole, outward static pressure is applied to the side wall of the slot hole to form a force balance, thereby forming a dense mud skin on the slot wall. The mud can penetrate into the stratum and attach to soil particles, thereby improving the stability of the soil layer through adhesion, thereby maintaining the stability of the slot wall.
[0038] Bentonite powder uses sodium-based bentonite with stronger hydration expansion ability. Compared with calcium-based and magnesium-based bentonite, sodium-based bentonite has better water retention and rheological properties, and better physical and chemical properties.
[0039] The admixture used is hydroxypropyl methylcellulose (HPMC) instead of the conventional carboxymethyl cellulose (CMC). The ability of hydroxypropyl methylcellulose to improve the mud colloid rate and water loss performance indicators is better than that of carboxymethyl cellulose. When added with a thickener, the mud viscosity and colloid rate can be increased, so that the mud has good sand carrying capacity, bonding ability and stability, ensuring the adsorption of quicksand and avoiding excessive precipitation of gravel at the bottom of the trough. At the same time, it can quickly consolidate to form a stable wall protection structure.
[0040] Soda ash is easily ionized and hydrolyzed in water. Soda ash is added to the mud to improve the hydration and dispersion properties of clay and to adjust the pH value of the mud. The pH value is generally required to be 8-10. Too low a pH value will reduce the stability of the mud and make it easy to precipitate, while too high a pH value will cause mud stratification.
[0041] A small amount of cement is added as a leak-proof agent to block the large pores and leakage channels in the formation, prevent large amounts of mud from leaking out, and at the same time make the formed wall-protecting mud skin stronger to avoid collapse.
[0042] Compared with the prior art, the wall protection slurry and construction method suitable for riverside geology described in the present invention have the following advantages:
[0043] (1) The slurry mix ratio developed by the present invention through experiments is suitable for weak strata with strong water absorption, high water permeability and high groundwater level, such as silty silty loam layers and fine sand layers, and effectively avoids the collapse and necking phenomenon in the trenching;
[0044] (2) The additive hydroxypropyl methylcellulose (HPMC) added to the mud wall of the present invention has better effect than the commonly used carboxymethyl cellulose (CMC), significantly increases the viscosity and yield value of the mud, improves the colloidal properties of the mud, reduces water loss, improves the suspension capacity of drilling cuttings and the wall solidification effect, and adds a small amount of cement to avoid a large amount of mud leakage from the formation;
[0045] (3) In construction sites with high groundwater levels, the present invention maintains the mud level more than 1 m above the groundwater level, and utilizes the head pressure formed by the high head difference inside and outside the slot hole to make the mud adhere to the slot wall, thereby improving the stability of the slot wall and gradually forming a thin and dense mud wall protective layer during construction. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0047] Figure 1 It is a schematic cross-sectional view of the mud wall protection described in an embodiment of the present invention.
[0048] Description of reference numerals:
[0049] 1. Guide trough; 2. Construction plane; 3. Mud level; 4. Groundwater level. DETAILED DESCRIPTION
[0050] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0051] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and the like are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", and the like may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0052] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0053] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.
[0054] The mix ratio of the mud of the present invention is given according to the foundation soil composition of the construction area of the Fenghuangjing Pump Station Reconstruction Project. First, the soil layer distribution of the buildings in the project area is surveyed, and sampling tests are carried out on each soil layer to determine the physical and mechanical properties of each soil layer. Then, according to the soil layer characteristics of the weakest stratum, combined with relevant construction specifications and field experience, the preliminary performance indicators of the mud are given (see Table 1).
[0055] Table 1 Bentonite slurry performance indicators
[0056]
[0057]
[0058] In order to determine the influence of each raw material on the mud performance, single factor experiments were carried out on bentonite content, soda ash content, hydroxypropyl methylcellulose (HPMC) content and cement content, and the differences in the measured mud performance indicators were compared.
[0059] Bentonite content experiment:
[0060] Prepare 1000ml of mud, set the stirring speed to 600r / min, stirring time to 1h, standing time to 1h, when the soda ash content is 0.2%, HPMC content is 0.01%, cement content is 0.05‰, bentonite content is 3%, 4%, 5%, 6%, 7% respectively, the mud properties are shown in Table 2.
[0061] Table 2 Mud properties with different bentonite mix ratios
[0062]
[0063] Soda ash content experiment:
[0064] Prepare 1000ml mud, set the stirring speed to 600r / min, stirring time to 1h, standing time to 1h, and when the bentonite content is 5%, the HPMC content is 0.01%, the cement content is 0.05‰, and the soda content is 0.05%, 0.1%, 0.2%, 0.3%, and 0.5%, the mud properties are shown in Table 3. In the experiment, the soda solution is prepared first, and then the bentonite is added to give full play to the hydration and dispersion properties of the soda.
[0065] Table 3 Mud properties with different soda ash mix ratios
[0066]
[0067] Hydroxypropyl methylcellulose content experiment:
[0068] Prepare 1000 ml of mud, set the stirring speed to 600 r / min, the stirring time to 1 h, and the standing time to 1 h. When the bentonite content is 5%, the soda ash content is 0.2%, the cement content is 0.05‰, and the hydroxypropyl methylcellulose content is 0.002%, 0.005%, 0.01%, 0.05%, and 0.1% respectively, the mud properties obtained are shown in Table 4.
[0069] Table 4 Mud properties with different HPMC mix ratios
[0070]
[0071] Cement content test:
[0072] Prepare 1000ml of mud, set the stirring speed to 600r / min, stirring time to 1h, standing time to 1h, when the bentonite content is 5%, the HPMC content is 0.01%, the soda ash content is 0.2%, and the cement contents are 0.006‰, 0.01‰, 0.05‰, 0.1‰, and 0.3‰ respectively, the mud properties are shown in Table 5.
[0073] Table 5 Mud properties with different cement mix ratios
[0074]
[0075]
[0076] Through the single-factor mud proportioning experiment, it can be found that the specific gravity and viscosity of the mud increase with the increase of bentonite content; the soda ash content has little effect on the specific gravity of the mud, significantly reduces the plastic viscosity of the mud, and has a certain effect on improving the pH value; hydroxypropyl methylcellulose has little effect on the specific gravity of the mud, greatly increases the viscosity of the mud, and greatly reduces the water loss and mud cake thickness; cement increases the specific gravity of the mud to a certain extent, and the increase in viscosity is more obvious.
[0077] Example 1
[0078] 52 kg of bentonite was mixed into water and stirred evenly to obtain mixed solution 1; 2.4 kg of soda ash, 0.25 kg of hydroxypropyl methylcellulose, 0.12 kg of thickener and 0.07 kg of cement were mixed into water and stirred until fully hydrated to obtain mixed solution 2; mixed solution 1 and mixed solution 2 were stirred evenly to obtain mud.
[0079] Comparative Example 1
[0080] 64 kg of bentonite was mixed into water and stirred evenly to obtain mixed solution 1; 2.1 kg of soda ash, 0.15 kg of hydroxypropyl methylcellulose, 0.18 kg of thickener and 0.1 kg of cement were mixed into water and stirred until fully hydrated to obtain mixed solution 2; mixed solution 1 and mixed solution 2 were stirred evenly to obtain mud.
[0081] Comparative Example 2
[0082] 40 kg of bentonite was mixed into water and stirred evenly to obtain mixed solution 1; 2.7 kg of soda ash, 0.35 kg of hydroxypropyl methylcellulose, 0.05 kg of thickener and 0.04 kg of cement were mixed into water and stirred until fully hydrated to obtain mixed solution 2; mixed solution 1 and mixed solution 2 were stirred evenly to obtain mud.
[0083] The slurry mix ratios of the above examples and comparative examples are shown in Table 6.
[0084] Table 6 Bentonite slurry mix ratio
[0085]
[0086] Mud properties of the above examples and comparative examples (see Table 7)
[0087] Table 7 Bentonite slurry properties under different mix ratios
[0088]
[0089] The hole cleaning parameters of the above embodiments and comparative examples (see Table 8)
[0090] Table 8 Bentonite slurry hole cleaning parameters under different mix ratios
[0091]
[0092] Test methods for each performance index:
[0093] Specific gravity: Pour the mud sample into the mud cup, flush with the cup mouth, drain the excess mud and air, slowly move the weight on the scale, when the bubble is in the center and the lever is horizontal, the scale value is the specific gravity.
[0094] Funnel viscosity: Block the outflow port at the bottom of the funnel with your finger, inject the mud sample into the funnel through the sieve until the liquid level reaches the bottom of the sieve, remove your finger and start the stopwatch. The time required for the sample to flow to the 1500ml mark in the measuring cup is the funnel viscosity.
[0095] Plastic viscosity: Pour the mud sample into the container until the liquid level reaches the scale line, rotate the drum at 600 min / r and 300 min / r respectively, and record the readings. The plastic viscosity can be calculated according to formula (1).
[0096] Dynamic shear force: The dynamic shear force can be calculated according to formula (2).
[0097] Static shear force: The mud sample is kept still for 10 seconds and 10 minutes respectively, and the maximum reading when it rotates at a speed of 3min / r is measured. The static shear force can be calculated according to formula (3).
[0098] Water loss and mud cake thickness: keep a certain volume of mud sample under specified air pressure for 30 minutes. The amount of filtrate flowing out is the water loss. Take out the sample, wash off the floating slurry, and measure the mud cake thickness.
[0099] pH: Dip the mud filtrate that has passed the water loss meter test and drop it in the middle of the pH test paper. Compare the stabilized color with the standard colorimetric card to get the pH value.
[0100] Sand content: Fill the mud to the mark on the sand content measuring tube, add clean water to the engraved line, block the tube mouth and shake it thoroughly, filter the solution through the screen, and mix the unfiltered solution with clean water. After shaking, filter again. Repeat the operation until the measuring tube is clean. The sand content on the screen is the sand content.
[0101] PV=Φ 600 -Φ 300 (1)
[0102] YP=0.511(2Φ 300 -Φ 600 ) (2)
[0103] G=0.511Φ3 (3)
[0104] In the formula, PV is the plastic viscosity, YP is the dynamic shear force, G is the static shear force, Φ 600 , Φ 300 , Φ3 are the readings on the dial when the rotation speed is 600min / r, 300min / r, and 3min / r respectively.
[0105] Mud supply and storage:
[0106] The mud supply system is mainly composed of bentonite warehouse, mud mixer, mud pump, mud pool, waste slurry pool, etc. Mud is made by mud mixer, and mud pump transports mud to each construction slot section. Mud pool and waste slurry pool are excavated and constructed, and their capacity needs to meet the requirements of mud storage and circulation. During the troughing process, the mud in the trough needs to be replaced, and the performance indicators of the mud are tested by the detection device. The unqualified mud is placed in the waste slurry pool for sedimentation. If it meets the slurry making standards, it can be pumped back to the mud pool for recycling by mud pump. The sediment at the bottom of the waste slurry pool is picked up by excavator, transported to the designated location by dump truck for storage, and corresponding environmental protection measures are taken.
[0107] The walls of the mud pool are built with bricks, and the bottom of the pool is poured with 10cm thick C15 concrete. The dimensions are 16×13×2m (length×width×depth), which can meet the mud demand for simultaneous construction of two trough sections. A waste slurry pool is set up near the mud pool with the same construction standards as the mud pool. The dimensions of the waste slurry pool are 12×8×2m (length×width×depth).
[0108] Mud construction method:
[0109] The construction site is leveled, the pile position of the cut-off wall is measured and located, holes are drilled and soil is taken at the pile position, and a guide groove 1 is constructed; the guide groove 1 includes a horizontal section and a vertical section, the horizontal section is arranged on the construction plane 2, the top surface of the horizontal section is 10 cm higher than the construction plane 2 on both sides, and the distance between the top surface of the horizontal section and the mud liquid surface 3 is 0.3-0.5 m to avoid overflow, and the vertical section is arranged in the slot hole, and the inner diameter of the vertical section corresponds to the inner diameter of the slot hole.
[0110] The prepared mud is pumped into the mud pool for standby use. The mud needs to be frequently stirred to keep it uniform and avoid sedimentation or segregation. The trenching equipment drills holes and injects mud to remove drilling debris. The mud level 3 is higher than the groundwater level 4 by more than 1.0m to maintain a high head difference inside and outside the trench.
[0111] Circulating mud: Inject mud into the slot hole, and use a mud pump to pump the mud containing suspended drilling cuttings in the slot hole from the drilling equipment into the waste mud pool for sedimentation treatment. During the slot construction process, due to the mixing of rock cuttings and the consumption of other treatment agents, the mud performance in the slot hole will gradually deteriorate, and slurry replacement treatment is required.
[0112] Take out the drilling equipment and install the steel cage and conduit in the slot.
[0113] Removing sediment from the bottom of the slot: Inject sedimentation treated slurry into the slot, and use a mud pump to pump the sediment from the bottom of the slot from the conduit into the waste slurry pool for sedimentation treatment.
[0114] Test the mud in the slot hole. The mud density in the slot hole is ≤1.15g / cm 3 , funnel viscosity is 32-50s, and sand content is ≤4%.
[0115] Drainage ditches are set up around the trough holes and mud pools to prevent large amounts of surface sewage or rainwater from flowing in and contaminating the mud.
[0116] During trenching construction, avoid loads and equipment near the trench wall that generate additional stress on the trench wall, reduce equipment vibration, and avoid trench wall collapse due to external forces.
[0117] Mud quality control:
[0118] 1. Test the performance index of fresh mud just prepared in the mixer. The sampling time is 200m after the mixer completes 3 Test once when the mud is being stirred;
[0119] 2. Test the performance index of the mud stored in the mud pool, with sampling time once every 24 hours;
[0120] 3. The mud that has been purified by slurry replacement needs to be tested for performance indicators before use. Samples should be taken from the mud pool to test relevant indicators. If the density of bentonite (mud density), funnel viscosity and sand content cannot meet the requirements, it is necessary to replace the qualified bentonite mud;
[0121] 4. Test the performance indicators of the mud in the tank, and take samples of the upper mud in the tank for testing when the tank reaches half its depth and near the end.
[0122] The control standards for the performance indicators of the mud in 1-2 above are shown in Table 9.
[0123] Table 9 Performance index control standards of fresh bentonite slurry on site
[0124] Performance Indicators <![CDATA[Density / (g / cm 3 )]]> Funnel viscosity / (s) mud 1.03~1.08 35~50
[0125] The control standards for the performance indicators of the mud in 3-4 above are shown in Table 10 (the sand content is measured using a sand content meter)
[0126] Table 10 Control standards for on-site bentonite slurry performance indicators
[0127] Performance Indicators <![CDATA[Density / (g / cm 3 )]]> Funnel viscosity / (s) Sand content / (%) mud ≤1.15 32~50 ≤4
[0128] Field Test:
[0129] Through on-site drilling, the mud with different mix ratios was tested. After the drilling was completed, the mud was circulated in the hole for 12 hours, and the changes in the hole wall were observed with an ultrasonic detector every 1 hour to check whether there were necking, hole collapse, etc. Then the hole cleaning test was carried out to clean out a large amount of sediment at the bottom of the trough, and at the same time, attention was paid to whether there were any abnormalities during the hole cleaning process. Since the mud was diluted during the hole cleaning process, the mud specific gravity decreased, which may cause the soil balance to be destroyed, resulting in hole collapse and neck shrinkage.
[0130] Comparing the test results of muds with different mix ratios, the mud in Example 1 has too high a specific gravity, which reduces the hole-making speed and makes it more difficult to clean the hole in the later stage; the mud in Example 2 has a slightly smaller specific gravity and too high a viscosity, which also does not meet the performance index requirements, and there is a lot of leakage after hole making, and there are signs of necking; the mud in Example 1 uses less material and has lower cost. It has a good effect in the test and no abnormal phenomenon occurs. The mud performance meets the construction requirements. In practical applications, it is recommended to appropriately increase the cement content to enhance the stability of the mud wall.
[0131] During the construction of the cut-off wall, no obvious hole collapse, neck shrinkage or leakage was found, and the construction effect was good.
[0132] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A wall protection slurry suitable for riverside geology, Features: The invention comprises the following components by weight: 51-53 kg bentonite, 2.3-2.5 kg soda ash, 0.36-0.38 kg hydroxypropyl methylcellulose, 0.10-0.14 kg thickener, 0.06-0.08 kg cement and 1000 kg water.
2. The wall protection mud suitable for riverside geology according to claim 1, Features: The following components are included by weight: 52 kg bentonite, 2.4 kg soda ash, 0.25 kg hydroxypropyl methylcellulose, 0.12 kg thickener, 0.07 kg cement, and 1000 kg water.
3. The wall protection mud suitable for riverside geology according to claim 1, Features: The bentonite is sodium bentonite; The thickener includes one or more of gypsum, ethoxylated sodium alkyl sulfide, and sodium dodecyl sulfonate.
4. A method for preparing wall-protecting mud suitable for riverside geology according to any one of claims 1 to 3, Features: The following steps are involved: S1: Mix bentonite into water and stir evenly to obtain a mixed solution 1; S2: mixing soda ash, hydroxypropyl methylcellulose, thickener and cement into water, stirring until fully hydrated, to obtain mixed solution 2; S3: Mix the mixed solution 1 and the mixed solution 2 to obtain slurry.
5. A construction method for wall protection slurry suitable for riverside geology according to any one of claims 1 to 3, Features: The following steps are involved: S1: Measure and locate the pile position of the cut-off wall, drill holes at the pile position, take soil, and construct the guide groove; S2: The trenching equipment drills a hole and injects the mud described in claims 1 to 3 to remove drilling debris, wherein the mud liquid level is more than 1.0 m above the groundwater level (4); S3: circulating the slurry; S4: Take out the drilling equipment and install the steel cage and the guide tube in the slot; S5: remove the sediment at the bottom of the slot; S6: Detecting the mud in the slot.
6. The construction method according to claim 5, Features: The guide groove (1) in S1 comprises a horizontal section and a vertical section. The horizontal section is arranged on the construction plane (2). The top surface of the horizontal section is 10 cm higher than the construction planes (2) on both sides. The distance between the top surface of the horizontal section and the mud liquid surface (3) is 0.3-0.5 m. The vertical section is arranged in the slot hole, and the inner diameter of the vertical section corresponds to the inner diameter of the slot hole.
7. The construction method according to claim 5, Features: Before the injection of the mud in S2, the following steps are also included: pumping the prepared mud into a mud pool, stirring the mud to keep the mud uniform.
8. A quality control method for wall protection slurry suitable for riverside geology according to any one of claims 1 to 3, Features: The specific control methods are as follows: S1: The performance index of the mud as described in claims 1-3 just prepared in the mixer is tested, and the sampling time is 160-240 minutes after the mixer is completed. 3 Test once when the mud is being stirred; S2: Testing the performance index of the mud stored in the mud pool, with sampling time once every 20-28 hours; S3: The mud that has been purified by mud replacement needs to be tested for performance indicators before use. Samples are taken from the mud pool to test relevant indicators. If the mud density, funnel viscosity and sand content of the mud cannot meet the requirements, it is necessary to replace the mud with qualified ones. S4: Testing the performance indexes of the mud in the tank, sampling and testing the upper mud in the tank when the tank is halfway deep and near the end.
9. The quality control method according to claim 8, Features: The sampling time in S1 is 200 minutes after the mixer completes 3 Test once when the mud is being stirred; The sampling time in S2 is once every 24 hours.
10. The quality control method according to claim 8, Features: The mud performance index in S1-S2 is: mud density 1.03-1.08g / cm 3 , funnel viscosity is 35-50s; The mud performance index in S3-S4 is: mud density ≤ 1.15g / cm 3 , funnel viscosity is 32-50s, and sand content is ≤4%.