Environment-friendly pet sand as well as preparation method and recycling method thereof

By combining high-silicon calcium-based solid waste with porous active materials, deodorants and microbial agents, environmentally friendly pet sand for particle size greater than 50, and recycling through anaerobic fermentation or high-temperature pyrolysis treatment, the traditional solution is solved The cost, poor effect and solid waste treatment of pet sand have been high, which has achieved efficient resource recycling and improved performance of environmentally friendly pet sand.

CN118947559APending Publication Date: 2024-11-15PANZHIHUA UNIV

Patent Information

Application Number
CN202411315328.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Traditional pet sand preparation costs are high, poor effect, large amounts are used, and difficult to recycle, and the problem of high-silicon calcium-based solid waste treatment has not been effectively solved.

Method used

High-silicon calcium-based solid waste is used as the particle core, and the surface is coated with mixed powder, including high-silicon calcium-based solid waste, porous active materials, deodorants and microbial agents, to prepare environmentally friendly pet sand for particle size greater than 50, and Recycling by anaerobic fermentation or high-temperature pyrolysis treatment.

Benefits of technology

It realizes the high value-added resource utilization of environmentally friendly pet sand, which has good water absorption, deodorization and agglomeration, reduces dependence on traditional non-renewable resources, reduces environmental costs, and transforms organic fertilizers. Recycling of resources is realized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118947559A_ABST
    Figure CN118947559A_ABST
Patent Text Reader

Abstract

The invention discloses environment-friendly pet sand as well as a preparation method and a recycling method thereof, and belongs to the field of solid waste resource utilization and new materials. The environment-friendly pet sand is specifically formed particles with the particle size larger than 50 meshes. The molded particles take high-silicon calcium-based solid waste with the particle size of 100-200 meshes as a particle core, and the surface of the particle core is coated with a layer of mixed powder; the mixed powder comprises the following components: 80-93% of high-silicon calcium-based solid waste with the particle size of less than 300 meshes, 5-10% of a porous active material, 1-5% of a deodorant and 1-5% of a microbial agent; the agglomerated blocky sand used by pets is prepared into an organic fertilizer through anaerobic fermentation or high-temperature pyrolysis. The environment-friendly pet sand is simple in preparation process and low in raw material cost, high value-added resource utilization of high-silicon calcium-based solid waste can be achieved, the water absorption rate of the environment-friendly pet sand is 51.1%-412.5%, the agglomeration rate is 100%, and the deodorization effect is larger than 98%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of solid waste resource utilization and new materials, and specifically relates to an environmentally friendly pet litter and a preparation method and a recycling method thereof. Background Art

[0002] In today's society, pets have become an indispensable member of many families, and the pet products market has also developed rapidly. Among them, pet litter is a necessity for pet life, and its demand is growing. However, most of the pet litter on the market currently uses non-renewable resources such as bentonite as the main raw material. The mining of bentonite not only causes damage to the environment, such as destroying land vegetation and causing soil erosion, but also its resource reserves are limited and it is difficult to meet long-term market demand. In addition, there are still some problems with traditional pet litter during use. For example, some pet litter has poor water absorption and deodorization properties, which can easily lead to an unsanitary living environment for pets and increase the risk of pets getting sick. At the same time, traditional pet litter is usually difficult to effectively handle after use, and a large amount of discarded pet litter is randomly discarded or landfilled, which not only occupies land resources, but also may cause pollution to the soil, water and atmospheric environment. With the continuous improvement of people's environmental awareness, the demand for environmentally friendly pet litter is becoming increasingly urgent.

[0003] On the other hand, the treatment of high-silicon calcium-based solid waste has always been a difficult problem faced by the industrial field. High-silicon calcium-based solid waste mainly comes from the production processes of metallurgy, chemical industry, building materials and other industries. These solid wastes contain a large amount of silicon, calcium and other elements. If they are not properly treated, they will cause serious harm to the environment. First, the accumulation of high-silicon calcium-based solid waste will occupy a large amount of land resources and affect the utilization value of the land. Secondly, the harmful substances in the solid waste may penetrate into the soil and water bodies with the erosion of rainwater, causing soil pollution and water pollution, and damaging the ecological environment. In addition, some high-silicon calcium-based solid wastes may also generate dust and pollute the atmospheric environment. Therefore, it is of great practical significance to find an effective method for the treatment of high-silicon calcium-based solid waste and realize the resource utilization of solid waste.

[0004] So far, there are no reports on the application of high-silicon calcium-based solid waste in the field of pet litter technology. How to combine high-silicon calcium-based solid waste with pet litter, while solving the problems of resource utilization of existing high-silicon calcium-based solid waste and the adverse effects of traditional pet litter on the environment, and improving the application performance of existing pet litter, is a new challenge facing researchers. Summary of the invention

[0005] The technical problems to be solved by the present invention are the high preparation cost, poor effect, large dosage and difficult recycling of traditional pet litter, as well as a new way to resource utilization of high-silicon-calcium-based solid waste.

[0006] The technical solution adopted by the present invention to solve the technical problem is:

[0007] In a first aspect, the present invention provides an environmentally friendly pet litter, specifically, formed particles with a particle size greater than 50 mesh; the formed particles use high-silicon calcium-based solid waste with a particle size of 100 to 200 mesh as the particle core, and the surface of the particle core is coated with a layer of mixed powder; the composition of the mixed powder is as follows by mass percentage: 80% to 93% of high-silicon calcium-based solid waste with a particle size less than 300 mesh, 5% to 10% of porous active material, 1% to 5% of deodorant, and 1% to 5% of microbial agent.

[0008] In the above-mentioned environmentally friendly pet litter, the high-silicon-calcium-based solid waste is at least one of phosphogypsum, flue gas desulfurization gypsum, titanium gypsum, phosphate tailings, vanadium-titanium magnetite tailings, iron tailings, copper tailings, lead-zinc tailings, coal gangue, fly ash, steel slag, and antimony tailings.

[0009] In the above-mentioned environmentally friendly pet litter, the porous active material is at least one of activated carbon, zeolite, cement, and slag powder.

[0010] In the above-mentioned environmentally friendly pet litter, the deodorant is at least one of castor oil zinc ester, soybean ethyl sulfate morpholine, chlorine dioxide, photocatalyst, methacrylate fatty alcohol, and wood acetic acid.

[0011] In the above-mentioned environmentally friendly pet litter, the microbial agent is at least one of photosynthetic bacteria, acetic acid bacteria, actinomycetes, lactic acid bacteria, yeasts and pseudomonas.

[0012] The water absorption rate of the environmentally friendly pet litter is 51.1% to 412.5%, the agglomeration rate is 100%, and the deodorization effect is greater than 98%.

[0013] In a second aspect, the present invention provides a method for preparing the above-mentioned environmentally friendly pet litter, comprising the following steps:

[0014] A. Dry the high-silicon calcium-based solid waste at 45°C to 90°C and then sieve;

[0015] A1. Obtain high-silicon calcium-based solid waste particles with a particle size of 100 to 200 mesh for standby use;

[0016] A2. The remaining particle size of high-silicon calcium-based solid waste is crushed to less than 300 mesh, and dried at 150-200°C to remove crystal water to obtain high-silicon calcium-based solid waste powder;

[0017] B. mixing the high-silicon calcium-based solid waste powder obtained in step A2, the porous active material, the deodorant and the microbial agent in proportion to obtain a mixed powder;

[0018] C. Rinse the high-silicon calcium-based solid waste particles obtained in step A1 with water to make them have water stains on their surfaces, use the water-carrying high-silicon calcium-based solid waste particles as particle cores, add the mixed powder obtained in step B, and perform disc granulation in coordination with mechanical vibration to obtain formed particles with a particle size greater than 50 mesh;

[0019] D. Dry the shaped particles obtained in step C at 100° C. to 150° C., cool them down, and then clean them to obtain environmentally friendly pet litter.

[0020] In the above preparation method, in step D, the cleaning method adopts the method of bottom blowing coordinated with negative pressure. During the cooling process of the formed particles, the dust is removed from the bottom of the particles by airflow. The bottom blowing airflow rate is 0.5 to 3 m / s. The cooling process maintains a negative pressure state, and the negative pressure intensity is 50 to 200 Pa.

[0021] In a third aspect, the present invention provides a method for recycling the above-mentioned environmentally friendly pet litter: the used environmentally friendly pet litter containing pet feces is prepared into organic fertilizer through anaerobic fermentation or high-temperature pyrolysis.

[0022] Furthermore, the anaerobic fermentation treatment is as follows: adding water to the agglomerated environmentally friendly pet litter containing pet feces at a solid-liquid ratio of 1:2 to 5, quickly stirring to disperse the lumpy sand, inoculating sludge or EM bacterial agent at 0.1% to 0.5%, and fully fermenting under anaerobic conditions for 15 to 25 days to obtain organic fertilizer.

[0023] Furthermore, the high-temperature pyrolysis treatment is: placing the used environmentally friendly pet litter under 200-800° C. for pyrolysis for 1-5 hours, and then rapidly cooling the temperature to obtain carbon-based organic fertilizer.

[0024] The beneficial effects of the present invention are as follows: in the preparation method of the environmentally friendly pet litter of the present invention, the high-silicon calcium-based solid waste is mechanically crushed to stimulate its gelling activity, and the existing crystal water components are stripped under high temperature conditions. The treated solid waste can react with water to undergo hydration reaction and quickly form agglomerates. The porous material is added mainly to increase the contact with pet feces during the use of the pet and to stop the emission of odor in time. The deodorant and microorganisms are added mainly to reduce the release of odor by chemical and microbial methods. The powder is compounded to form an outer wrapping material, and the core material of the pet litter is granular high-silicon calcium-based solid waste. The high-silicon calcium-based solid waste particles with moist surfaces react quickly with the powder. The powder is strongly adsorbed on the surface of the particles through a hydration reaction, resulting in the gradually enhanced hydration performance of the wrapped powder from the inside to the outside. After removing the powder that is not adsorbed on the surface, the environmentally friendly pet litter is obtained. The used pet litter contains a large amount of organic matter components, which can be prepared into organic fertilizer by fermentation and pyrolysis. The whole process realizes the high added value resource utilization and closed cycle of solid waste.

[0025] From an environmental perspective: This method can reduce dependence on traditional non-renewable resources and reduce environmental costs in the production process of pet litter. As an industrial waste, high-silicon calcium-based solid waste has a wide range of sources and a large amount. By rationally treating and utilizing these solid wastes, they can be converted into valuable pet litter products to achieve resource recycling. Secondly, pet litter prepared using high-silicon calcium-based solid waste can have good water absorption, deodorization and agglomeration properties. Elements such as silicon and calcium in high-silicon calcium-based solid waste can interact with other additives to form pet litter with specific structures and properties. By adding an appropriate amount of binder and deodorant, pet litter can have better water absorption and deodorization effects, providing a clean and comfortable living environment for pets.

[0026] From the perspective of sustainable development. This method has important strategic significance. On the one hand, this method can realize the resource utilization of industrial waste, reduce pollution to the environment, and meet the strategic requirements of national sustainable development. On the other hand, this method can provide a new source of environmentally friendly raw materials for the pet products industry and promote the sustainable development of the pet products industry. At the same time, subsequent fertilizer treatment can convert used pet litter into organic fertilizer, provide nutrients for agricultural production, and realize the recycling of resources. In addition, this method can also drive the development of related industries, such as solid waste treatment industry, pet products industry and agriculture, and create more employment opportunities and economic benefits.

[0027] The preparation process of the environmentally friendly pet litter of the present invention is simple, the cost of raw materials is low, and high value-added resource utilization of high-silicon calcium-based solid waste can be achieved. The water absorption rate of the environmentally friendly pet litter is 51.1%-412.5%, the agglomeration rate is 100%, the deodorization effect is greater than 98%, the water absorption performance is significant, the agglomeration performance is good, and the deodorization performance is significant; the prepared organic fertilizer has a significant planting effect. The environmentally friendly pet litter of the present invention and its preparation method and recycling method can not only solve the problem of treating high-silicon calcium-based solid waste, but also provide a new source of environmentally friendly raw materials for pet litter, realize the recycling of resources, and have broad development prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A flow chart of a method for preparing and recycling environmentally friendly pet litter;

[0029] Figure 2 To implement the performance test results of Case 1 phosphogypsum environmentally friendly pet litter;

[0030] Figure 3 The performance test results of environmentally friendly pet litter from vanadium-titanium magnet tailings were implemented in Case 2;

[0031] Figure 4This is the performance test results of the implementation case 3 coal gangue environmentally friendly pet litter. DETAILED DESCRIPTION

[0032] The technical solution of the present invention can be specifically implemented in the following manner.

[0033] The present invention provides a method for preparing environmentally friendly pet litter from high-silicon calcium-based solid waste and subsequent fertilizer production. The specific process is as follows: Figure 1 As shown. The method dries and crushes high-silicon calcium-based solid waste to less than 300 meshes, strips off crystal water at 150-200°C, and fully mixes 80%-93% of the crushed high-silicon calcium-based solid waste, 5%-10% of porous active materials, 1%-5% of deodorants and 1%-5% of microbial agents under dry conditions to form a mixed powder; sieves out 100-200 mesh high-silicon calcium-based solid waste particles, rinses them with water and directly puts them into the mixed powder, granulates them by mechanical vibration, screens out molded particles larger than 50 meshes, dries them at 100°C-150°C, and re-enters the granulation stage for particles smaller than 50 meshes. After drying, the particles are cooled and cleaned to obtain environmentally friendly pet litter. The environmentally friendly pet litter has a water absorption rate of 51.1%-412.5%, a reunion rate of 100%, and a deodorization effect of more than 98%. The agglomerated sand after pet use is prepared into organic fertilizer through anaerobic fermentation or high-temperature pyrolysis, and the entire process achieves complete resource utilization.

[0034] The technical solution and effects of the present invention are further illustrated below through practical examples.

[0035] Example

[0036] 1. Preparation of environmentally friendly pet litter

[0037] (1) Pretreatment of high-silicon calcium-based solid waste: The high-silicon calcium-based solid waste is dried and sieved; high-silicon calcium-based solid waste particles with a particle size of 100 to 200 mesh are obtained for standby use; the high-silicon calcium-based solid waste with other particle sizes is crushed to less than 300 mesh, dried and stripped of crystal water, and high-silicon calcium-based solid waste powder is obtained; the specific process is shown in Table 1.

[0038] Table 1 Pretreatment process

[0039] Example 1 Example 2 Example 3 High silicon calcium based solid waste Phosphogypsum Vanadium Titanium Magnetite Tailings Coal Gangue Drying temperature 45℃ 90℃ 60℃ Drying temperature 150℃ 200℃ 180℃

[0040] (2) Compounding of mixed powder: High silicon calcium-based solid waste powder, porous active material, deodorant and microbial agent are uniformly mixed according to the proportions in Table 2 to obtain mixed powder.

[0041] Table 2 Mixed powder components / %

[0042]

[0043]

[0044] (3) Granulation and cleaning: rinse the high-silicon calcium-based solid waste particles with water to make them have water stains on their surface, use the water-carrying high-silicon calcium-based solid waste particles as the particle core, add the mixed powder, and use mechanical vibration to granulate; screen, and re-enter the granulation stage for particles smaller than 50 meshes, and dry the formed particles larger than 50 meshes. After cooling, use bottom blowing airflow to coordinate negative pressure conditions to clean the dust to obtain environmentally friendly pet litter. The specific process is shown in Table 3.

[0045] Table 3 Granulation and cleaning process

[0046] Example 1 Example 2 Example 3 Drying temperature 100℃ 150℃ 130℃ Bottom blowing air flow rate 0.5m / s 3m / s 1.5m / s Negative pressure intensity 50Pa 200Pa 100Pa

[0047] 2. Performance test of environmentally friendly pet litter

[0048] Example 1 Performance test results of phosphogypsum environmentally friendly pet litter Figure 2 As shown in the figure, it can be seen that: the release concentration of toxic and harmful elements is low through the leaching toxicity experiment, among which the P content is about 0.5 mg / L, the F content is about 0.1 mg / L, and the Zn / Mn / Pb content is close to 0, which does not affect the use of pets; the water absorption rate is 300% to 400%, which has a significant water absorption rate; through the agglomeration effect analysis, it is found that the agglomeration effect is significant (the agglomeration test is the agglomeration density; the agglomeration strength test is the ratio of the mass of the agglomerated cat litter that falls from a height of 1m to the original mass); the deodorization effect is simulated using ammonia water, and it is found that the deodorization effect is significant.

[0049] Example 2 Performance test results of vanadium-titanium magnet tailings environmentally friendly pet litter Figure 3 As shown in the figure, it can be seen that: the release concentration of toxic and harmful elements is low through the leaching toxicity experiment, among which the P content is about 0.1 mg / L, the F content is about 0.01 mg / L, and the Zn content is about 0.01 mg / L, which does not affect the use of pets; the water absorption rate is 200%~250%, which has a significant water absorption rate; the agglomeration effect analysis found that the agglomeration effect is significant; the deodorization effect is simulated using ammonia water, and it is found that the deodorization effect is significant.

[0050] Example 3 Performance test results of coal gangue environmentally friendly pet litter Figure 4 As shown in the figure, it can be seen that: the release concentration of toxic and harmful elements is low through the leaching toxicity experiment, among which the P content is about 0.02 mg / L, the F content is about 0.01 mg / L, and the Zn content is about 0.05 mg / L, which does not affect the use of pets; the water absorption rate is 100% to 150%, and it has a significant water absorption rate; the agglomeration effect analysis found that the agglomeration effect is significant; the deodorization effect is simulated using ammonia water, and it is found that the deodorization effect is significant.

[0051] 3. Recycling of environmentally friendly pet litter

[0052] (1) Recycling method

[0053] Example 1 Recycling of environmentally friendly pet litter containing phosphogypsum: Collect pet litter containing pet feces after use; ① Prepare organic fertilizer using fermentation technology: Add water to the agglomerated litter containing pet feces at a solid-liquid ratio of 1:2, stir quickly and evenly to disperse the blocky cat litter, and inoculate 0.1% sludge; fully ferment under anaerobic conditions for 15 days to become organic fertilizer A1; ② Prepare carbon-based organic fertilizer A2 using high-temperature pyrolysis technology: Place the used cat litter at 200°C for pyrolysis for 1 hour, and obtain carbon-based organic fertilizer after rapid cooling.

[0054] Example 2 Recycling of environmentally friendly pet litter from vanadium-titanium magnet tailings: Collect pet litter containing pet feces after use; ① Prepare organic fertilizer using fermentation technology: Add water to the agglomerated litter containing pet feces at a solid-liquid ratio of 1:5, stir quickly and evenly to disperse the blocky cat litter, and inoculate 0.1% of the purchased EM bacterial agent; fully ferment under anaerobic conditions for 25 days to become organic fertilizer B1; ② Prepare carbon-based organic fertilizer using high-temperature pyrolysis technology: Place the used cat litter at 800°C for pyrolysis for 5 hours, and obtain carbon-based organic fertilizer B2 after rapid cooling.

[0055] Example 3 Recycling of environmentally friendly pet litter made of coal gangue: Collect pet litter containing pet feces after use; ① Prepare organic fertilizer using fermentation technology: Add water to the agglomerated litter containing pet feces at a solid-liquid ratio of 1:3, stir quickly and evenly to disperse the blocky cat litter, and inoculate 0.1% of the purchased EM bacterial agent; fully ferment under anaerobic conditions for 25 days to become organic fertilizer C1; ② Prepare carbon-based organic fertilizer using high-temperature pyrolysis technology: Pyrolyze the used cat litter at 600°C for 3 hours, and obtain carbon-based organic fertilizer C2 after rapid cooling.

[0056] (2) Fertilizer efficiency testing

[0057] The fertilizer efficiency test was conducted in a vegetable garden. The test soil was a vegetable garden soil with a high degree of maturity. The test seeds were Chinese cabbage seeds. The vegetable garden field plot experiment set up three treatments: no fertilizer control, anaerobic fermentation organic fertilizer, and high temperature pyrolysis organic fertilizer. Each treatment was repeated 3 times, arranged in random blocks, and the plot area was 2m 2 , 200 seeds were sown in each area. Among them, the organic fertilizer fertilization method was carried out according to the conventional chemical fertilizer application method, and the fertilizer and water management during the test was carried out according to the routine. The test ended on the 20th day and the index was measured. The organic fertilizers obtained by anaerobic fermentation and pyrolysis treatment of the environmentally friendly pet litter recycled in the embodiment of the present invention all meet the organic fertilizer standards (NY / T-525-2021), and the test results are shown in Table 4.

[0058] Table 4 Fertilizer efficiency index

[0059]

Claims

1. Environmentally friendly pet litter, characterized by: The molded particles have a particle size greater than 50 meshes; the molded particles have high-silicon calcium-based solid waste with a particle size of 100 to 200 meshes as the particle core, and the surface of the particle core is coated with a layer of mixed powder; the components of the mixed powder are as follows by mass percentage: 80% to 93% of high-silicon calcium-based solid waste with a particle size less than 300 meshes, 5% to 10% of porous active materials, 1% to 5% of deodorants, and 1% to 5% of microbial agents.

2. The environmentally friendly pet litter according to claim 1, characterized in that: The high-silicon-calcium-based solid waste is at least one of phosphogypsum, flue gas desulfurization gypsum, titanium gypsum, phosphate tailings, vanadium-titanium magnetite tailings, iron tailings, copper tailings, lead-zinc tailings, coal gangue, fly ash, steel slag, and antimony tailings.

3. The environmentally friendly pet litter according to claim 1, characterized in that: The porous active material is at least one of activated carbon, zeolite, cement and slag powder.

4. The environmentally friendly pet litter according to claim 1, characterized in that: The deodorant is at least one of castor oil zinc alcoholate, soybean ethyl sulfate morpholine, chlorine dioxide, photocatalyst, methacrylate fatty alcohol, and wood acetic acid.

5. The environmentally friendly pet litter according to claim 1, characterized in that: The microbial agent is at least one of photosynthetic bacteria, acetic acid bacteria, actinomycetes, lactic acid bacteria, yeasts and pseudomonas.

6. The environmentally friendly pet litter according to claim 1, characterized in that: Its water absorption rate is 51.1% to 412.5%, its agglomeration rate is 100%, and its deodorization effect is greater than 98%.

7. The method for preparing the environmentally friendly pet litter according to any one of claims 1 to 6, characterized in that: The steps include: A. Dry the high-silicon calcium-based solid waste at 45°C to 90°C and then sieve; A1. Obtain high-silicon calcium-based solid waste particles with a particle size of 100 to 200 mesh for standby use; A2. The remaining particle size of high-silicon calcium-based solid waste is crushed to less than 300 mesh, and dried at 150-200°C to remove crystal water to obtain high-silicon calcium-based solid waste powder; B. mixing the high-silicon calcium-based solid waste powder obtained in step A2, the porous active material, the deodorant and the microbial agent in proportion to obtain a mixed powder; C. Rinse the high-silicon calcium-based solid waste particles obtained in step A1 with water to make them have water stains on their surfaces, use the water-carrying high-silicon calcium-based solid waste particles as particle cores, add the mixed powder obtained in step B, and perform disc granulation in coordination with mechanical vibration to obtain formed particles with a particle size greater than 50 mesh; D. Dry the shaped particles obtained in step C at 100° C. to 150° C., cool them down, and then clean them to obtain environmentally friendly pet litter.

8. The method for preparing the environmentally friendly pet litter according to claim 7, characterized in that: In step D, the dust removal method adopts the method of bottom blowing coordinated with negative pressure. During the cooling process of the formed particles, the dust is removed from the bottom of the particles by airflow. The bottom blowing airflow velocity is 0.5 to 3 m / s. The cooling process maintains a negative pressure state, and the negative pressure intensity is 50 to 200 Pa.

9. The method for recycling environmentally friendly pet litter according to any one of claims 1 to 6, characterized in that: The environmentally friendly pet litter containing pet excrement after use is prepared into organic fertilizer through anaerobic fermentation treatment or high-temperature pyrolysis treatment.

10. The method for recycling environmentally friendly pet litter according to claim 9, characterized in that: The anaerobic fermentation treatment comprises: adding water to the agglomerated environmentally friendly pet litter containing pet feces at a solid-liquid ratio of 1:2-5, rapidly stirring to disperse the agglomerated sand, inoculating sludge or EM bacterial agent at 0.1%-0.5%, and fully fermenting under anaerobic conditions for 15-25 days to obtain organic fertilizer; The high-temperature pyrolysis treatment is as follows: placing the used environmentally friendly pet litter under the condition of 200-800° C. for pyrolysis for 1-5 hours, and then rapidly cooling it down to obtain a carbon-based organic fertilizer.

Citation Information

Patent Citations

  • Citrus pomace-based cat litter and making method thereof

    CN109169312A

  • Resourceful treatment method for waste residues containing heavy metals and cat litter prepared by resourceful treatment method

    CN117694253A

  • Method for preparing adsorbing material from industrial and agricultural solid wastes

    CN118384857A

  • Animal breeding bedding material

    JP2020103221A

  • Toilet litter for domestic animals

    RU2158078C1

Cited By

  • Environment-friendly cat litter capable of comprehensively utilizing copper tailings and preparation method of environment-friendly cat litter