UHPC formula and preparation method

Through the formulation and stirring preparation methods of materials such as cement, microsilicon powder, steel fiber modified, nanosilicon dioxide and ultra-high molecular weight polyethylene fiber modified, the complex problem of UHPC production process is solved and high pressure resistance is achieved UHPC with strength and low curing temperature is suitable for building curtain wall materials and is suitable for large-scale industrial production.

CN118930150AInactive Publication Date: 2024-11-12YUNNAN ZHUHUI BUILDING MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411141593.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing UHPC production process is complex, which makes it rare in practical applications, and lacks a production method that is easy to obtain raw materials and simple to process.

Method used

UHPC is prepared by stirring through a mixer using cement, microsilicon powder and steel fiber modifications, nanosilicon dioxide and ultra-high molecular weight polyethylene fiber modifications, silica sand, water reducing agent and water. The specific steps include cement, After mixing silica sand, water reducer and water, microsilicon powder, steel fiber modified, nanosilica and ultra-high molecular weight polyethylene fiber modified are added in sequence to obtain UHPC with high compressive strength.

Benefits of technology

It realizes the efficient and simple preparation process of UHPC, is suitable for building curtain wall materials, has the characteristics of high compressive strength and low curing temperature, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930150A_ABST
    Figure CN118930150A_ABST
Patent Text Reader

Abstract

The UHPC formula comprises the following raw materials in parts by weight: 650 to 670 parts of cement, 200 to 210 parts of silica fume and a steel fiber modifier, 150 to 180 parts of nano silicon dioxide and an ultra-high molecular weight polyethylene fiber modifier, 850 to 890 parts of silica sand, 10 to 12 parts of a water reducing agent and 150 to 180 parts of water. The preparation method of the UHPC comprises the following steps: putting the cement, the silica sand, the water reducing agent and the water into a stirrer, and stirring for 5 minutes to obtain cement paste; continuously stirring, sequentially adding the micro silicon powder, the steel fiber modifier, the nano silicon dioxide, the ultra-high molecular weight polyethylene fiber modifier and the water into the cement paste, and then stirring for 4 minutes to obtain the UHPC. According to the UHPC formula, the raw materials are rich and easy to obtain, and the UHPC formula is suitable for large-scale industrial production; the preparation method of the UHPC is simple and efficient in process; the UHPC prepared by the method has the characteristics of high compressive strength and low curing temperature, and can be applied to building curtain wall materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of concrete, and in particular to a UHPC formula and a preparation method. Background Art

[0002] Ultra-High Performance Concrete (UHPC) is also called Ultra-High Performance Fibre Reinforced Concrete (UHPFRC) because it generally needs to be mixed with steel fibers or high-strength polymer fibers. UHPC is different from traditional high-strength concrete (HSC) and steel fiber concrete (SFRC), nor is it the high-strength of the traditional "high-performance concrete (HPC)". It is a new type of cement-based structural engineering material with clear performance indicators. It is a new type of cement-based composite material developed in the past three decades. It has ultra-high mechanical properties and durability, and has good toughness, bonding properties, and impact and fatigue resistance. With the advancement and development of green concrete engineering materials, ultra-high strength and high-performance concrete has attracted great attention in improving the environment, improving economic benefits, and solving difficult problems in engineering.

[0003] UHPC generally needs to have the following characteristics: it is a cement-based composite material with the best gradation of its constituent material particles; the water-cement ratio is less than 0.25, and it contains a high proportion of fine short steel fiber reinforcements; the compressive strength is not less than 150MPa; it has toughness in a tensile state, and after cracking, it still maintains a tensile strength of not less than 5MPa; it has a non-connected pore structure inside, and has a high ability to resist gas and liquid infiltration. Compared with traditional concrete and high-performance concrete (HPC), its durability can be greatly improved.

[0004] UHPC has great potential in various fields due to its superior performance compared to ordinary concrete, but it is relatively rare in practical applications because the production process of UHPC is very complicated, so its production is limited.

[0005] In summary, there is an urgent need to propose a UHPC formula with readily available raw materials and a simple production method. Summary of the invention

[0006] In order to solve the problem that the existing UHPC manufacturing process is very complicated, the present invention proposes a UHPC formula, the raw materials of which include: cement, microsilica powder and steel fiber modification, nano silicon dioxide and ultra-high molecular weight polyethylene fiber modification, silica sand, water reducing agent and water.

[0007] In a preferred embodiment of the present invention, the raw materials, calculated in parts, include: 650-670 parts of cement, 200-210 parts of microsilica powder and modified steel fiber, 150-180 parts of nano silicon dioxide and modified ultra-high molecular weight polyethylene fiber, 850-890 parts of silica sand, 10-12 parts of water reducer and 150-180 parts of water.

[0008] In a preferred embodiment of the present invention, the particle size of the microsilica powder is 50-100 nm.

[0009] Furthermore, the preparation method of microsilica powder and steel fiber modified product is as follows: dissolve 100 parts of microsilica powder in 200 parts of anhydrous ethanol and 10 parts of water, add 2 parts of KH550, and then heat to 70°C, keep warm for 1 hour, dissolve 100 parts of steel fiber into the above-mentioned mixed solution, stir for 2 hours, and then dry or bake to obtain microsilica powder and steel fiber modified product.

[0010] In a preferred embodiment of the present invention, the particle size of nano-silicon dioxide is 1-50 nm.

[0011] Furthermore, the preparation method of microsilica powder and steel fiber modified product is as follows: add 1 part of DL602 to 35 parts of nano-silica in 200 parts of anhydrous ethanol and 10 parts of water, then heat to 80°C and keep warm for 2 hours, add 120 parts of ultra-high molecular weight polyethylene fiber into the above-mentioned mixture, stir for 2 hours, and then dry or bake to obtain nano-silica and ultra-high molecular weight polyethylene fiber modified products.

[0012] In a preferred embodiment of the present invention, the method for preparing UHPC comprises the following steps:

[0013] S1. Put cement, silica sand, water reducing agent and water into a mixer and stir for 5 minutes to obtain cement slurry;

[0014] S2. Continue stirring, and add microsilica powder and steel fiber modification, nano silicon dioxide and ultra-high molecular weight polyethylene fiber modification, and water into the cement slurry in turn, and then stir for 4 minutes to obtain UHPC.

[0015] Furthermore, the cubic compressive strength of UHPC is not less than 250 MPa.

[0016] Furthermore, the curing temperature of UHPC is 80-100°C.

[0017] Furthermore, UHPC is used in building curtain wall materials.

[0018] The implementation of the present invention has the following beneficial effects:

[0019] The UHPC formula of the present invention has abundant and readily available raw materials and is suitable for large-scale industrial production; the preparation method of UHPC has a simple and efficient process; the UHPC prepared by the method has the characteristics of high compressive strength and low curing temperature, and can be suitable for use as a building curtain wall material. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 This is a flow chart of the method for producing UHPC provided by the present invention. DETAILED DESCRIPTION

[0022] The following will be combined with the accompanying drawings in the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The invention provides a UHPC formula, the raw materials of which include cement, microsilica powder and steel fiber modification, nano silicon dioxide and ultra-high molecular weight polyethylene fiber modification, silica sand, water reducing agent and water.

[0024] The raw materials, calculated in parts, include: 650-670 parts of cement, 200-210 parts of microsilica powder and steel fiber modification, 150-180 parts of nano silicon dioxide and ultra-high molecular weight polyethylene fiber modification, 850-890 parts of silica sand, 10-12 parts of water reducer and 150-180 parts of water.

[0025] The preparation method of microsilica powder and steel fiber modified product is as follows: 100 parts of microsilica powder are dissolved in 200 parts of anhydrous ethanol and 10 parts of water, 2 parts of KH550 are added, and then heated to 70°C, kept warm for 1 hour, 100 parts of steel fiber are dissolved in the above-mentioned mixed solution, stirred for 2 hours, and then dried or baked to obtain microsilica powder and steel fiber modified product. Among them, the particle size of microsilica powder is 50-100nm.

[0026] The preparation method of microsilica powder and steel fiber modified product is as follows: 35 parts of nano silicon dioxide are added to 200 parts of anhydrous ethanol and 10 parts of water, 1 part of DL602 is added, and then heated to 80°C, kept warm for 2 hours, 120 parts of ultra-high molecular weight polyethylene fiber are added to the above mixture, stirred for 2 hours, and then air-dried or baked to obtain nano silicon dioxide and ultra-high molecular weight polyethylene fiber modified product. Among them, the particle size of nano silicon dioxide is 1-50nm.

[0027] See also Figure 1 , Figure 1 The present invention provides a flow chart of the method for preparing UHPC; the method for preparing UHPC comprises the following steps:

[0028] S1. Put 650 parts of cement, 860 parts of silica sand, 10 parts of water reducer and 100 parts of water into a mixer and stir for 5 minutes to obtain cement slurry;

[0029] S2. Continue stirring, and add 200 parts of microsilica powder and steel fiber modification, 170 parts of nano-silica and ultra-high molecular weight polyethylene fiber modification, and 60 parts of water into the cement paste in sequence, and then stir for 4 minutes to obtain UHPC.

[0030] The UHPC prepared by the above method is used for building curtain wall materials, with a cubic compressive strength of not less than 250MPa and a curing temperature of 80-100°C.

[0031] Example 1

[0032] A method for preparing UHPC comprises the following steps:

[0033] S1. Put 650 parts of cement, 850 parts of silica sand, 10 parts of water reducer and 100 parts of water into a mixer and stir for 5 minutes to obtain cement slurry;

[0034] S2. Continue stirring, and add 200 parts of microsilica powder and modified steel fiber, 150 parts of nano-silicon dioxide and modified ultra-high molecular weight polyethylene fiber, and 50 parts of water into the cement paste in sequence, and then stir for 4 minutes to obtain UHPC.

[0035] Example 2

[0036] A method for preparing UHPC comprises the following steps:

[0037] S1. Put 660 parts of cement, 850 parts of silica sand, 11 parts of water reducer and 120 parts of water into a mixer and stir for 5 minutes to obtain cement slurry;

[0038] S2. Continue stirring, and add 210 parts of microsilica powder and modified steel fiber, 160 parts of nano-silica and modified ultra-high molecular weight polyethylene fiber, and 50 parts of water into the cement paste in sequence, and then stir for 4 minutes to obtain UHPC.

[0039] Example 3

[0040] A method for preparing UHPC comprises the following steps:

[0041] S1. Put 660 parts of cement, 870 parts of silica sand, 12 parts of water reducer and 125 parts of water into a mixer and stir for 5 minutes to obtain cement slurry;

[0042] S2. Continue stirring, and add 200 parts of microsilica powder and steel fiber modification, 160 parts of nano-silica and ultra-high molecular weight polyethylene fiber modification, and 40 parts of water into the cement slurry in sequence, and then stir for 4 minutes to obtain UHPC.

[0043] Example 4

[0044] A method for preparing UHPC comprises the following steps:

[0045] S1. Put 670 parts of cement, 880 parts of silica sand, 12 parts of water reducer and 140 parts of water into a mixer and stir for 5 minutes to obtain cement slurry;

[0046] S2. Continue stirring, and add 210 parts of microsilica powder and steel fiber modification, 180 parts of nano-silica and ultra-high molecular weight polyethylene fiber modification, and 40 parts of water into the cement slurry in sequence, and then stir for 4 minutes to obtain UHPC.

[0047] Example 5

[0048] A method for preparing UHPC comprises the following steps:

[0049] S1. Put 670 parts of cement, 890 parts of silica sand, 12 parts of water reducer and 150 parts of water into a mixer and stir for 5 minutes to obtain cement slurry;

[0050] S2. Continue stirring, and add 210 parts of microsilica powder and modified steel fiber, 180 parts of nano-silica and modified ultra-high molecular weight polyethylene fiber, and 30 parts of water into the cement paste in sequence, and then stir for 4 minutes to obtain UHPC.

[0051] Example 6

[0052] A method for preparing UHPC comprises the following steps:

[0053] S1. Put 670 parts of cement, 890 parts of silica sand, 12 parts of water reducer and 150 parts of water into a mixer and stir for 5 minutes to obtain cement slurry;

[0054] S2. Continue stirring, and add 150 parts of microsilica powder and steel fiber modification, 120 parts of nano-silica and ultra-high molecular weight polyethylene fiber modification, and 15 parts of water into the cement slurry in sequence, and then stir for 4 minutes to obtain UHPC.

[0055] Compressive strength test:

[0056] The UHPC prepared in the above six embodiments was prepared into a cubic workpiece of a specified size. After curing at a curing temperature of 100° C. for 2 days, a compressive strength test was performed. The test results are shown in Table 1 below:

[0057] Table 1 Compressive strength test results

[0058]

[0059] From the above results, it can be seen that the cubic compressive strength of the five groups of UHPC (Examples 1-5) prepared by the formula and preparation method of the technical solution is above 250 MPa, among which the cubic compressive strength of Example 5 is the highest. The cubic compressive strength of the UHPC prepared by Example 6 using other proportion formulas is only 102 MPa, which is very different from the UHPC obtained by the other five examples. Therefore, the formula ratio of this solution is the best solution.

[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A UHPC formula, characterized in that: The raw materials include: cement, microsilica powder and steel fiber modification, nano silicon dioxide and ultra-high molecular weight polyethylene fiber modification, silica sand, water reducing agent and water.

2. The UHPC formulation according to claim 1, characterized in that The raw materials, calculated in parts, include: 650-670 parts of cement, 200-210 parts of microsilica powder and steel fiber modification, 150-180 parts of nano silicon dioxide and ultra-high molecular weight polyethylene fiber modification, 850-890 parts of silica sand, 10-12 parts of water reducer and 150-180 parts of water.

3. The UHPC formulation according to claim 1, characterized in that The particle size of the microsilica powder is 50-100 nm.

4. The UHPC formulation according to claim 3, characterized in that The preparation method of the microsilica powder and steel fiber modified product is as follows: dissolve 100 parts of microsilica powder in 200 parts of anhydrous ethanol and 10 parts of water, add 2 parts of KH550, and then heat to 70°C, keep warm for 1 hour, dissolve 100 parts of steel fiber into the above-mentioned mixed solution, stir for 2 hours, and then dry or bake to obtain the microsilica powder and steel fiber modified product.

5. The UHPC formulation according to claim 1, characterized in that The particle size of the nano silicon dioxide is 1-50nm.

6. The UHPC formulation according to claim 5, characterized in that The preparation method of the microsilica powder and steel fiber modified product is as follows: 35 parts of nano-silica are dissolved in 200 parts of anhydrous ethanol and 10 parts of water, 1 part of DL602 is added, and then the mixture is heated to 80°C and kept warm for 2 hours, 120 parts of ultra-high molecular weight polyethylene fibers are added to the mixed solution, stirred for 2 hours, and then air-dried or baked to obtain nano-silica and ultra-high molecular weight polyethylene fiber modified products.

7. The UHPC formulation according to any one of claims 1 to 6, characterized in that: The preparation method of UHPC comprises the following steps: S1. Put cement, silica sand, water reducing agent and water into a mixer and stir for 5 minutes to obtain cement slurry; S2. Continue stirring, and add microsilica powder and steel fiber modification, nano silicon dioxide and ultra-high molecular weight polyethylene fiber modification, and water into the cement slurry in turn, and then stir for 4 minutes to obtain UHPC.

8. The UHPC formulation according to any one of claim 7, characterized in that: The cubic compressive strength of the UHPC is not less than 250 MPa.

9. The UHPC formulation according to any one of claim 7, characterized in that: The curing temperature of the UHPC is 80-100°C.

10. The UHPC formulation according to any one of claim 7, characterized in that: The UHPC is used as a building curtain wall material.

Citation Information

Patent Citations

  • Steel fiber high-strength concrete and preparation method thereof

    CN111517718A

  • Preparation method of ultra-high performance concrete

    CN115159929A

  • Formula and preparation method of novel nanocomposite UHPC

    CN115611565A

  • Surface-modified steel fiber, modification method and concrete based on steel fiber

    CN117800641A

  • Sports safety checker with vital information

    KR102296726B1