Concrete workpiece and preparation method thereof

By using dry ice particles in concrete parts to react with the gelling material, the internal pore structure and chemical carbon sequestration are formed, and the problem of low carbon sequestration in the prior art is solved, and efficient carbon dioxide fixation and cost reduction effects are achieved.

CN118930156APending Publication Date: 2024-11-12HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411166930.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing carbon dioxide curing methods have low carbon sequestration, limited carbon sequestration effect, and high cost and high energy consumption.

Method used

Using the preparation method of concrete parts, cementitious materials, aggregates, water and dry ice particles are used as raw materials, and cured and formed by stirring and printing. Dry ice sublimation produces gaseous carbon dioxide and reacts with concrete to form internal pore structure and chemical carbon sequestration to improve Carbon sequestration amount.

Benefits of technology

It effectively increases the amount of carbon sequestration, reduces the atmospheric carbon dioxide concentration, slows down global warming, and has low preparation costs, and the materials can be degraded and does not affect the secondary utilization of construction waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930156A_ABST
    Figure CN118930156A_ABST
Patent Text Reader

Abstract

The invention belongs to the related technical field of building materials, and discloses a concrete workpiece and a preparation method thereof.The concrete workpiece is prepared from a cementing material, aggregate, water and dry ice particles as raw materials through stirring and then curing forming in a mold or curing forming after printing; wherein the dry ice particles comprise a packaging material and dry ice, the dry ice is packaged into a particle form by the packaging material, the dry ice is sublimated into gaseous carbon dioxide in the curing forming process, and the carbon dioxide can break through the packaging material and react with raw materials of the concrete workpiece to achieve carbon sequestration. Carbon dioxide is used as a preparation raw material in the form of dry ice particles, uniform distribution of the dry ice particles in the raw material can be realized, and the characteristic that air pressure in the dry ice particles is increased due to sublimation of the dry ice is utilized, so that the dry ice can break through a packaging material in the form of gaseous carbon dioxide to flow into the material, and absorption of carbon dioxide is realized; and the carbon sequestration amount is effectively increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field related to building materials, and more specifically, relates to a concrete component and a preparation method thereof. Background Art

[0002] At present, global carbon consumption is increasing, and carbon dioxide emissions are also rising rapidly. 2 It is one of the main greenhouse gases, which can absorb and radiate heat energy from the ground, causing the temperature of the earth's surface to rise and trigger global warming. With human activities, global warming is becoming more and more serious, changing human lifestyles while posing a great threat to the entire ecosystem. 2 , achieving carbon neutrality is imminent.

[0003] Patent CN103030166A proposes a carbon dioxide solidification method, which converts carbon dioxide into carbonate for solidification through carbonate precipitation. However, this method is not suitable for large-scale solidification, and the raw material cost is high. The solidified product occupies land resources like slag. CN110357473A discloses a carbonization-enhanced recycled aggregate and its preparation method and application, which uses construction waste and some additives to make recycled aggregate, and then pre-cures and carbonizes the aggregate. The disadvantage is that the carbonization gas is a high-concentration CO 2 , high maintenance pressure, high energy consumption, high cost, and limited carbon fixation. Most of the existing carbon dioxide fixation methods have the problems of low carbon fixation and limited carbon fixation effect. Summary of the invention

[0004] In view of the above defects or improvement needs of the prior art, the present invention provides a concrete component and a preparation method thereof, which solves the problems of low carbon fixation amount and limited carbon fixation effect in most existing carbon dioxide solidification methods, and can achieve effective carbon fixation inside the concrete component and increase the carbon fixation amount.

[0005] To achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided a concrete component, which is prepared by first mixing cementitious material, aggregate, water and dry ice particles as raw materials, and then curing and forming in a mold or curing and forming after printing, wherein the dry ice particles include packaging material and dry ice, and the dry ice is packaged into particle form by the packaging material. During the curing process, the dry ice sublimates into gaseous carbon dioxide, and the carbon dioxide can break through the packaging material and react with the raw materials of the concrete component to achieve carbon fixation.

[0006] According to the concrete component provided by the present invention, the interior of the concrete component also has a pore structure formed by the flow of carbon dioxide.

[0007] According to the concrete component provided by the present invention, the proportions of the raw materials are: 1 part of water, 2 parts of cementitious material, 6 parts of aggregate and 0.2-0.4 parts of dry ice.

[0008] According to the concrete component provided by the present invention, the packaging material is a degradable material; the degradable material is one of polylactic acid, ethylene / carbon monoxide copolymer, and vinyl / vinyl ketone copolymer.

[0009] According to the concrete component provided by the present invention, the cementitious material is one of lime, gypsum and cement; the particle size of the dry ice particles is less than or equal to 2 mm; the particle size of the aggregate is 0.5-2 mm; and the aggregate is quartz sand or artificial sand.

[0010] According to the concrete part provided by the present invention, when the concrete part is prepared by curing and forming after printing, the raw materials also include an accelerating setting agent.

[0011] According to the concrete member provided by the present invention, the concrete member is a cuboid and is used for building a wall;

[0012] Alternatively, the concrete member is a cuboid and a sawtooth structure is provided on one side surface of the cuboid; the concrete member is used for building a wall and the sawtooth structure is located on the inner side of the wall.

[0013] According to another aspect of the present invention, a method for preparing a concrete component is provided, for preparing any of the above concrete components, the method comprising:

[0014] S1, mixing and stirring a cementitious material, an aggregate and water to obtain a concrete slurry;

[0015] S2, adding dry ice particles to the concrete slurry and stirring evenly to obtain a concrete raw material;

[0016] S3, pouring the concrete raw material into a mold to form a concrete blank; or forming a concrete blank by 3D printing the concrete raw material;

[0017] S4, curing and shaping the concrete blank to obtain a concrete product.

[0018] According to the method for preparing a concrete component provided by the present invention, S1, S2 and S3 are performed in an environment with a temperature less than or equal to 18°C.

[0019] According to the method for preparing a concrete part provided by the present invention, the proportion of the amount of dry ice particles added in S2 is obtained specifically by the following method:

[0020] Analyzing the components of the cementitious material and the hydration reactions of the components, obtaining the types of components that can absorb carbon dioxide in the hydration reaction as carbon-fixing components, and obtaining the mass proportion of the carbon-fixing components in the cementitious material;

[0021] According to the reaction formula of the carbon-fixing component and carbon dioxide during the hydration reaction, and the mass proportion of the carbon-fixing component in the cementitious material, the mass proportion of carbon dioxide required for the reaction in the cementitious material is obtained;

[0022] The addition ratio of the dry ice particles is obtained according to the mass ratio of the carbon dioxide required for the reaction in the gelling material.

[0023] In general, compared with the prior art, the above technical solutions conceived by the present invention provide concrete parts and preparation methods thereof:

[0024] 1. Carbon dioxide is used as a raw material in the form of dry ice particles. The dry ice particles can be evenly distributed in the raw materials by mixing and stirring the raw materials. The dry ice sublimation increases the internal pressure of the dry ice particles, so that during the curing and forming process of the concrete parts, the dry ice can break through the packaging material in the form of gaseous carbon dioxide and flow into the material, so that all parts inside the material will react with carbon dioxide to absorb carbon dioxide. Not only can the strength of the parts be evenly improved through the carbonization reaction with carbon dioxide, but also the carbon fixation effect can be achieved inside the concrete parts, and the carbon fixation amount can be effectively increased;

[0025] 2. Set up the CO formed after dry ice sublimation 2 A part of it reacts chemically with the cementitious material (chemical carbon fixation), and another part is directly sealed in the pores of the concrete in gaseous form (physical carbon fixation), further increasing the amount of carbon fixation. 2 , has the effect of reducing atmospheric CO 2 The content of CO 2 The connected pores produced by the circulation have a noise reduction effect, achieving green and low-carbon and noise reduction effects;

[0026] 3. The dry ice particles are wrapped with degradable materials. After the buildings where the concrete parts are used are demolished, it will not affect the secondary utilization of construction waste and has good environmental performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a structural schematic diagram of a concrete component provided by the present invention;

[0028] Figure 2 It is another structural schematic diagram of the concrete component provided by the present invention;

[0029] Figure 3 It is a schematic diagram of another application structure of the concrete member provided by the present invention;

[0030] Figure 4 It is a schematic diagram of the method for preparing the concrete component provided by the present invention. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0032] See also Figure 1 The first embodiment of the present invention provides a concrete component. The concrete component is prepared by first mixing cementitious material, aggregate, water and dry ice particles as raw materials, and then curing and forming in a mold or curing and forming after printing. The dry ice particles include packaging material and dry ice. The dry ice is packaged into a particle form by the packaging material. During the curing process, the dry ice sublimates into gaseous carbon dioxide. The carbon dioxide can break through the packaging material and react with the raw materials of the concrete component to achieve carbon fixation.

[0033] In this embodiment, carbon dioxide is used as a raw material in the form of dry ice particles to prepare a concrete product. The dry ice particles are first mixed with other raw materials and then solidified to form a concrete product. Specifically, the initial concrete blank can be formed by a mold or 3D printing, and the concrete blank can be solidified to obtain the final concrete product.

[0034] This embodiment uses dry ice particles as raw materials. The dry ice particles will sublime into gaseous carbon dioxide after leaving the dry ice preparation conditions. The packaging material that wraps the dry ice outside the dry ice particles can be a low-toughness material, and the packaging material can be broken under a preset air pressure; therefore, as the dry ice inside the dry ice particles sublimates, when the pressure of the gaseous carbon dioxide reaches the preset air pressure, the gaseous carbon dioxide can break through the packaging material.

[0035] Since the mixing time of raw materials is short and the solidification time is long during the preparation of concrete parts, and the dry ice particles can only break through the packaging material when the air pressure inside reaches the preset air pressure, the dry ice encapsulated in the dry ice particles mainly breaks through the packaging material in the form of gaseous carbon dioxide during the solidification stage. The carbon dioxide will flow inside the part before the concrete is completely solidified. The solidification process of concrete is accompanied by the hydration reaction of the cementitious material, which can react with carbon dioxide at the same time. For example, C in the cementitious material 2 S.C.3 S and some hydration products will react with CO 2 The reaction produces silica gel and CaCO 3 , thereby achieving the effect of absorbing and fixing carbon dioxide.

[0036] In this embodiment, carbon dioxide is used as a preparation raw material in the form of dry ice particles. The dry ice particles can be evenly distributed in the raw materials by mixing and stirring the raw materials. The characteristic of dry ice sublimation that the internal air pressure of the dry ice particles increases is utilized, so that during the curing and forming process of the concrete component, the dry ice can break through the packaging material in the form of gaseous carbon dioxide and flow into the interior of the material, so that all parts inside the material will react with the carbon dioxide to absorb the carbon dioxide. Not only can the strength of the component be evenly improved through the carbonization reaction with carbon dioxide, but also a carbon fixation effect can be achieved inside the concrete component, and the carbon fixation amount can be effectively increased.

[0037] This embodiment can reduce the concentration of carbon dioxide in the atmosphere by fixing carbon, thereby slowing down the trend of global warming and combating climate change. The prepared concrete parts can be used as building materials without occupying additional land resources. The raw materials for preparing the concrete parts are widely available and relatively common, and the preparation cost is low.

[0038] Furthermore, the interior of the concrete part also has a pore structure formed by the flow of carbon dioxide. 2 Part of it reacts chemically with the cementitious material (chemical carbon fixation), and part of it is directly sealed in the pores of the concrete in gaseous form (physical carbon fixation). 2 In addition, there is excess CO 2 , this part of CO 2 It will flow inside the concrete during the curing process, thus forming a large number of interconnected pores, i.e., pore structures, inside which CO can be fixed. 2 , thereby further increasing the amount of carbon fixation; this embodiment fixes CO 2 , has the effect of reducing atmospheric CO 2 The content of CO 2 The connected air holes created by the circulation have a noise reduction effect, achieving green and low-carbon and noise reduction effects.

[0039] This embodiment considers designing a building concrete component that integrates carbon fixation and noise reduction. Carbon dioxide is first pre-packaged in a low-toughness packaging material, and then mixed into the concrete to fix it in the component, which can effectively achieve the effect of carbon fixation. At the same time, carbon dioxide diffuses during the concrete solidification process to form a large number of interconnected pores. When sound waves propagate in the component, a large amount of energy is consumed, which has a noise reduction effect. The carbon fixation and noise reduction component uses chemical and physical methods to fix CO2 There are a lot of interconnected pores inside, which can effectively solve the current greenhouse effect problem and is an environmentally friendly and green building material. 2 Part of it reacts with the concrete, and part of it remains in the pores inside the concrete. Even if the building reaches the end of its service life and is demolished, only part of the CO is released. 2 .

[0040] Furthermore, the proportion of each raw material is: 1 part water, 2 parts cementitious material, 6 parts aggregate and 0.2-0.4 parts dry ice. That is, the mass ratio of water to cementitious material is 1:2; the mass ratio of water to aggregate is 1:6; the mass ratio of water to dry ice is 1:0.4-1:0.2. The mass ratio of water, cementitious material and aggregate can form a concrete component with good performance. The mass ratio of dry ice comprehensively considers chemical carbon fixation and physical carbon fixation, can meet the needs of chemical carbon fixation and can form a suitable pore ratio inside the concrete component.

[0041] Furthermore, the packaging material is a degradable material; the degradable material is one of polylactic acid, ethylene / carbon monoxide copolymer (E / CO), and vinyl / vinyl ketone copolymer (Ecolyte). These materials are degradable plastics and can be made into capsules to wrap dry ice. The sublimation temperature of dry ice is -78.5°C, that is, dry ice can sublimate into gas at room temperature, break through the outer plastic capsule, and then diffuse inside the workpiece. The dry ice particles used in this embodiment are wrapped with degradable materials, which can effectively improve the utilization rate of dry ice and reduce costs. After the building is demolished, it will not affect the secondary utilization of construction waste, and the environmental protection performance is good.

[0042] Furthermore, the cementitious material is one of lime, gypsum, and cement; the cementitious material can be a common material in concrete preparation, and can undergo carbonization reaction with carbon dioxide during hydration, and is not specifically limited. The particle size of the dry ice particles is less than or equal to 2 mm; the particle size of the aggregate is 0.5-2 mm; the aggregate is quartz sand or artificial sand. The particle size of the dry ice particles is preferably smaller than the particle size of the aggregate, so as to avoid the formation of large pores at the position of the dry ice particles when the dry ice sublimates, thereby affecting the performance of the product.

[0043] Furthermore, when the concrete part is prepared by curing after printing, the raw material also includes an accelerating agent. When the part is prepared by 3D printing, an accelerating agent can be added to the raw material, and the slurry after adding the accelerating agent and stirring and mixing is used for printing, so that printing and forming can be achieved. Furthermore, 0.04-0.16 parts of accelerating agent can be added.

[0044] Furthermore, the quick-setting agent can also accelerate the hardening speed of concrete, that is, the curing speed, which is conducive to achieving the corresponding hardening strength before the carbon dioxide diffuses to the surface of the product, thereby avoiding the formation of pores on the surface of the product and affecting the performance. When using a mold to prepare a product, a quick-setting agent can also be added to accelerate the forming, which is not specifically limited.

[0045] In some specific embodiments, reference Figure 1 The concrete component is a rectangular parallelepiped and is used for building a wall.

[0046] In other embodiments, reference Figure 2 and Figure 3 The concrete component is a rectangular parallelepiped and a sawtooth structure is provided on one side surface of the rectangular parallelepiped. The concrete component is used for building a wall and the sawtooth structure is located on the inner side of the wall.

[0047] For example, the concrete parts in this embodiment can be carbon-fixing bricks. There are two types of carbon-fixing bricks: one is a regular rectangular block, which is a common type and is used on the outside of the wall; the other is a sound-absorbing type with a serrated surface on one side of the rectangular block, which is used on the inside of the wall. The serrated surface can reduce the reflection and escape of sound waves to achieve the effect of sound absorption, providing an environmentally friendly and noise-reducing material for modern buildings.

[0048] The bricks made in this embodiment are divided into two types. The first type is a rectangular block, which has the characteristics of carbon fixation and noise reduction. The second type has one side configured to be serrated. Due to the characteristics of its structure, even if a part of the sawtooth of the sound wave is reflected, it will hit the adjacent sawtooth again, and the sound wave will be absorbed again, ultimately achieving the effect of preventing the sound wave from escaping. It has the characteristics of carbon fixation, sound absorption and noise reduction.

[0049] This embodiment 2 provides a method for preparing a concrete component, referring to Figure 4 The preparation method is used to prepare the concrete component described in any one of the above embodiments, and the preparation method comprises:

[0050] S1, mixing and stirring a cementitious material, an aggregate and water to obtain a concrete slurry;

[0051] S2, adding dry ice particles to the concrete slurry and stirring evenly to obtain a concrete raw material;

[0052] S3, pouring the concrete raw material into a mold to form a concrete blank; or forming a concrete blank by 3D printing the concrete raw material;

[0053] S4, curing and shaping the concrete blank to obtain a concrete product.

[0054] In this embodiment, dry ice and concrete slurry are stirred at the same time to prevent uneven gas diffusion; and the cementitious material, water and aggregate are first stirred evenly, and then the dry ice particles are added and stirred evenly, which can reduce the exposure time of the dry ice particles and help delay the sublimation of the dry ice particles, thereby preventing a large amount of dry ice from sublimating into carbon dioxide and escaping from the concrete parts before the curing and forming step. Concrete blanks can be prepared by molds or 3D printing. Mold preparation is to pour the concrete raw materials into the mold and slowly solidify and form them in the mold. 3D printing is to pass the concrete raw materials into the 3D printing equipment, prepare the concrete blank by printing, and then solidify and form the printed concrete blank. After curing and forming, the concrete parts are finally obtained.

[0055] When S3 is forming concrete blanks by 3D printing the concrete raw materials, correspondingly, S1 or S2 further includes: adding a corresponding mass portion of an accelerating setting agent.

[0056] Furthermore, S1, S2 and S3 are operated in an environment with a temperature of 18°C ​​or less. S1, S2 and S3 can be performed in a workshop with a temperature of 18°C ​​or less and in a closed environment, i.e., doors and windows are closed. It has been verified that a temperature of 18°C ​​or less is conducive to slowing down the sublimation rate of dry ice and ensuring that dry ice does not escape during the mixing of concrete slurry.

[0057] Furthermore, considering the sublimation speed of dry ice and the forming temperature of concrete, the operating environment temperature of S1, S2 and S3 can be 10-18°C.

[0058] Furthermore, the proportion of the amount of dry ice particles added in S2 is obtained in the following manner:

[0059] Analyzing the components of the cementitious material and the hydration reactions of the components, obtaining the types of components that can absorb carbon dioxide in the hydration reaction as carbon-fixing components, and obtaining the mass proportion of the carbon-fixing components in the cementitious material;

[0060] According to the reaction formula of the carbon-fixing component and carbon dioxide during the hydration reaction, and the mass proportion of the carbon-fixing component in the cementitious material, the mass proportion of carbon dioxide required for the reaction in the cementitious material is obtained;

[0061] The addition ratio of the dry ice particles is obtained according to the mass ratio of the carbon dioxide required for the reaction in the gelling material.

[0062] Furthermore, the mass proportion of dry ice particles should be slightly greater than the mass proportion of carbon dioxide required for the reaction in the cementitious material; so that the excess carbon dioxide in addition to chemical carbon fixation can form a pore structure in the concrete component, so that the concrete component can simultaneously increase the carbon fixation amount through physical carbon fixation and have a noise reduction function.

[0063] In some specific embodiments, the concrete parts may be carbon-fixing noise reduction bricks, which are prepared by mold preparation. The specific preparation method is:

[0064] Step 1: Mix water, cementitious material and aggregate according to mass proportions to obtain concrete slurry;

[0065] Specifically, aggregate and cement can be mixed according to mass fractions, stirred evenly, and then water of corresponding mass fractions is added thereto and stirred to form concrete slurry;

[0066] Step 2: Add dry ice particles of corresponding mass fraction into the concrete slurry and stir evenly to form concrete raw materials;

[0067] Accelerators of corresponding mass fractions may be selectively added;

[0068] Step 3: Pour concrete raw materials into the mold;

[0069] Step 4: After the raw materials are added, cover the mold top cover and solidify it into shape to obtain the carbon-fixing noise reduction brick.

[0070] The carbon-fixing noise-reducing brick is made by a mold. The above mold is divided into two types, one is used to make regular rectangular carbon-fixing noise-reducing bricks, such as Figure 1 , another one is used to make carbon-fixed noise-reducing bricks with sound-absorbing effect, such as Figure 2 .

[0071] In some other embodiments, the carbon-fixing noise reduction brick is prepared by a 3D printing method, comprising the following steps:

[0072] Step 1: Mix water, cementitious material and aggregate according to mass proportions to obtain concrete slurry;

[0073] Step 2: Add dry ice particles and accelerating agent in corresponding mass fractions to obtain concrete raw materials;

[0074] Step 3: The 3D printer completes the printing work and obtains the concrete blank;

[0075] Step 4: The concrete blank is solidified and formed to obtain a carbon-fixing noise-reducing brick.

[0076] Among them, the above 3D printed bricks are divided into two shapes. One is used to make regular rectangular carbon-fixing noise-reducing bricks such as Figure 1 , another type of carbon-fixing noise-reducing bricks with sound-absorbing properties, such as Figure 2 During the construction of the house, Figure 1 The bricks shown are used on the outdoor side to reduce noise. Figure 2 The bricks shown are used on one side of the room to absorb sound and reduce noise. Figure 3 shown.

[0077] In some specific embodiments, the cementitious material is cement, and the reaction of cement in hydration process mainly absorbing carbon dioxide is analyzed, that is, the chemical carbon fixation is mainly the cement hydration product Ca(OH) 2 With CO 2 The following reaction occurs:

[0078] Ca(OH) 2 +CO 2 →CaCO 3 ↓+H 2 O (1)

[0079] Furthermore, the mass proportion of carbon dioxide required for the reaction in cement is calculated as follows:

[0080] Analysis of the main mineral components of cement: 3CaO·SiO 2 (37%-60%), 2CaO·SiO 2 (15%-37%), 3CaO·Al 2 O 3 (7%-15%) and 4CaO·Al 2 O 3 ·Fe 2 O 3 (10%-18%).

[0081] The cement hydration reaction is as follows:

[0082] 2(3CaO·SiO 2 )+6H 2 O→3CaO·2SiO 2 ·3H 2 O+3Ca(OH) 2 (2)

[0083] 2(2CaO·SiO 2 )+4H 2 O→3CaO·2SiO 2 ·3H 2 O+Ca(OH) 2 (3)

[0084] 3CaO·Al 2 O 3 +6H 2 O→3CaO·Al 2 O 3 6H 2 O (4)

[0085] 4CaO·Al 2 O 3 ·Fe2 O 3 +7H 2 O→3CaO·Al 2 O 3 6H 2 O+3CaO·Fe 2 O 3 ·H 2 O (5)

[0086] It can be seen that the carbon fixation component in cement is mainly 3CaO·SiO 2 and 2CaO·SiO 2 According to 100g cement, the four main minerals 3CaO·SiO 2 ,2CaO·SiO 2 、3CaO·Al 2 O 3 and 4CaO·Al 2 O 3 ·Fe 2 O 3 Take 50g, 30g, 10g, and 10g respectively.

[0087] The molar masses M of the components are: M(3CaO·SiO 2 )=228g,M(2CaO·SiO 2 )=172g,M(Ca(OH) 2 )=74g,M(CO 2 )=44g;

[0088] Then the amount n of each component substance in the reaction is: n(3CaO·SiO 2 )=50 / 228mol→n 1 (Ca(OH) 2 )=75 / 228mol;

[0089] n(2CaO·SiO 2 )=30 / 172mol→n 2 (Ca(OH) 2 )=15 / 172mol;

[0090] n(Ca(OH) 2 )=n 1 (Ca(OH) 2 )+n 2 (Ca(OH) 2 )=0.41616mol;

[0091] According to formula (1), the consumption of CO 2 The amount of substance:

[0092] n(CO 2 )=0.41616mol, so CO 2 The mass of is 0.41616*44=18.31g; this mass is the mass of carbon dioxide required for the reaction when 100g of cement is added.

[0093] According to equations (1), (2), and (3), the CO involved in the chemical reaction is calculated. 2 There are 18.31g. Due to the different mineral components of different cements, the absorbed CO 2 There is a difference. At the same time, some carbon dioxide will be physically sealed in concrete products. Based on this, the mass of dry ice particles is set at 0.1-0.2 of the mass of cement, that is, the raw material ratio is: 1 part water, 2 parts cement, 6 parts aggregate, 0.2-0.4 parts dry ice. When adding accelerator, 0.04-0.16 parts of accelerator can be added.

[0094] That is, when the cementitious material is cement, the mass ratio of carbon dioxide required for the reaction in the cement is for:

[0095]

[0096] Among them, m 1 3CaO·SiO 2 The mass percentage in cement is the mass percentage; m 2 2CaO·SiO 2 The mass percentage of dry ice particles added to cement should be slightly greater than

[0097] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A concrete part, It is characterized in that The concrete is prepared by first mixing cementitious material, aggregate, water and dry ice particles as raw materials, and then curing and forming in a mold or curing and forming after printing. The dry ice particles include packaging material and dry ice. The dry ice is packaged into particle form by the packaging material. During the curing process, the dry ice sublimates into gaseous carbon dioxide. The carbon dioxide can break through the packaging material and react with the raw materials of the concrete component to achieve carbon fixation.

2. The concrete article according to claim 1, It is characterized in that The interior of the concrete component also has a pore structure formed by the flow of carbon dioxide.

3. The concrete article according to claim 1, It is characterized in that The proportions of each raw material are: 1 part water, 2 parts cementitious material, 6 parts aggregate and 0.2-0.4 parts dry ice.

4. The concrete article according to any one of claims 1 to 3, It is characterized in that The packaging material is a degradable material; the degradable material is one of polylactic acid, ethylene / carbon monoxide copolymer, and vinyl / vinyl ketone copolymer.

5. The concrete article according to any one of claims 1 to 3, It is characterized in that The cementitious material is one of lime, gypsum and cement; the particle size of the dry ice particles is less than or equal to 2 mm; the particle size of the aggregate is 0.5-2 mm; and the aggregate is quartz sand or artificial sand.

6. The concrete article according to any one of claims 1 to 3, It is characterized in that When the concrete part is prepared by curing and forming after printing, the raw materials also include an accelerating setting agent.

7. The concrete article according to any one of claims 1 to 3, It is characterized in that The concrete parts are rectangular parallelepiped and are used for wall construction; Alternatively, the concrete member is a cuboid and a sawtooth structure is provided on one side surface of the cuboid; the concrete member is used for building a wall and the sawtooth structure is located on the inner side of the wall.

8. A method for preparing a concrete part, It is characterized in that Used to prepare the concrete part according to any one of claims 1 to 7, the preparation method comprising: S1, mixing and stirring a cementitious material, an aggregate and water to obtain a concrete slurry; S2, adding dry ice particles to the concrete slurry and stirring evenly to obtain a concrete raw material; S3, pouring the concrete raw material into a mold to form a concrete blank; or forming a concrete blank by 3D printing the concrete raw material; S4, curing and shaping the concrete blank to obtain a concrete product.

9. The method for preparing a concrete component according to claim 8, It is characterized in that S1, S2 and S3 operate in an environment with a temperature less than or equal to 18°C.

10. The method for preparing a concrete component according to claim 8, It is characterized in that The proportion of dry ice particles added in S2 is obtained in the following way: Analyzing the components of the cementitious material and the hydration reactions of the components, obtaining the types of components that can absorb carbon dioxide in the hydration reaction as carbon-fixing components, and obtaining the mass proportion of the carbon-fixing components in the cementitious material; According to the reaction formula of the carbon-fixing component and carbon dioxide during the hydration reaction, and the mass proportion of the carbon-fixing component in the cementitious material, the mass proportion of carbon dioxide required for the reaction in the cementitious material is obtained; The addition ratio of the dry ice particles is obtained according to the mass ratio of the carbon dioxide required for the reaction in the gelling material.