Ultralow-carbon thermal insulation mortar and preparation method thereof
By using recycled concrete powder and carbonization curing technology in traditional insulation mortars, combined with polystyrene foam particles and polypropylene fibers, the problems of large consumption and low permeability of traditional insulation mortars are solved, and a new insulation with low carbon footprint is prepared. Mortar improves its mechanical and impermeability resistance, achieving building energy conservation and environmental protection.
Patent Information
- Application Number
- CN202411112385.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional insulation mortars have problems such as large cement consumption and low permeability, making it difficult to effectively achieve building energy conservation and emission reduction.
Recycled concrete powder is used to replace some cement clinker, and combined with carbonization and curing technology, polystyrene foam particles and polypropylene fibers are used to improve the crack resistance and permeability of the mortar and reduce carbon emissions.
A new insulation mortar with extremely low carbon footprint was prepared, which improved the mechanical properties and impermeability of the mortar, reduced the amount of cement used, and achieved resource conservation and environmental protection.
Smart Images

Figure CN118930181A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to an ultra-low carbon thermal insulation mortar and a preparation method thereof. Background Art
[0002] In the field of construction, thermal insulation materials play a vital role. As a key thermal insulation material, thermal insulation mortar is used for thermal insulation and heat insulation of building walls, roofs and other parts. It is of great significance to improve the energy-saving performance of buildings, ensure indoor comfort and reduce energy consumption. With global warming and increasingly prominent energy issues, building energy conservation has become a consensus and urgent need of the international community.
[0003] In response to the "dual carbon target" strategy, energy conservation and emission reduction in the construction industry is imperative. Among them, improving the thermal performance of exterior walls is one of the important measures to achieve building energy conservation. Insulation mortar using polystyrene foam particles as fine aggregate is a commonly used insulation material because of its good thermal performance and easy preparation. However, traditional insulation mortar has the problems of high cement consumption and low impermeability. Summary of the invention
[0004] The purpose of the present invention is to overcome at least one of the defects of the above-mentioned prior art and provide an ultra-low carbon thermal insulation mortar and a preparation method thereof. Recycled concrete powder has been proven to have a certain volcanic ash reaction and can be used as an auxiliary cementitious material to reduce the use of cement clinker. Due to the large amount of calcium materials contained, recycled concrete powder also has great carbon fixation potential. At the same time, through carbonization curing thermal insulation mortar, CO2 can react with cement hydration products in the pore fluid, and finally generate calcium carbonate on the surface of the mortar to fill the pores, thereby improving the mechanical properties and impermeability of the mortar.
[0005] The present invention is based on the traditional polystyrene thermal insulation mortar technology, further adding polypropylene fibers to improve its crack resistance, using recycled concrete powder to replace part of the cement clinker, and adopting carbonization curing technology to improve its anti-permeability and reduce its carbon emissions. Thus, a new thermal insulation mortar with an extremely low carbon footprint is prepared.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] One of the purposes of the present invention is to provide an ultra-low carbon thermal insulation mortar, comprising the following components in parts by weight: 400-700 parts of ordinary Portland cement; 300-600 parts of recycled micropowder; 600-800 parts of water; 90-125 parts of polystyrene foam particles; 20-25 parts of polypropylene fibers; 1-2 parts of air entraining agent; and 1-2 parts of foam stabilizer.
[0008] Furthermore, the ordinary Portland cement is PO 42.5 grade ordinary Portland cement, which meets the requirements of GB / T175-2007 "General Purpose Portland Cement".
[0009] Furthermore, the mixing water is ordinary tap water with a temperature not exceeding 40°C.
[0010] Furthermore, the recycled micropowder is recycled concrete powder, and its particle size distribution is similar to that of cement, and its particle size is not greater than 75 μm, meeting the requirements of JG-T 573-2020 "Recycled Micropowder for Concrete and Mortar".
[0011] Furthermore, the polystyrene foam particles are formed by mixing equal masses of 0.5-1 mm polystyrene foam particles, 1-2 mm polystyrene foam particles and 2-5 mm polystyrene foam particles. Preferably, the polystyrene foam particles have an average particle size of 0.5-5 mm, are smooth spherical particles, and have a bulk density of 21.10 kg / m 3 .
[0012] Further, the polypropylene fiber has an aspect ratio of 333 and a tensile strength of 400-500 MPa. Preferably, the polypropylene fiber has a length of about 6 mm, a diameter of about 18 μm, a tensile strength of 400 MPa, and a specific gravity of 0.90.
[0013] Furthermore, the air entraining agent is one or more of industrial α-sodium sulfonate, sodium alcohol ether sulfate or sodium dodecyl sulfate, meeting the requirements of GB 8076-2008 "Concrete Admixtures", preferably industrial α-sodium sulfonate.
[0014] Furthermore, the foam stabilizer is one or more of hydroxypropyl methylcellulose, calcium stearate or tea saponin, meeting the requirements of GB 8076-2008 "Concrete Admixtures". The foam stabilizer is preferably hydroxypropyl methylcellulose, more preferably hydroxypropyl methylcellulose with a viscosity of 200,000.
[0015] The second object of the present invention is to provide a method for preparing the ultra-low carbon thermal insulation mortar as described above, comprising the following steps:
[0016] S1. Mixing ordinary Portland cement, recycled concrete powder and part of water, stirring evenly to obtain a first mixture;
[0017] S2, stirring the air-entraining agent and part of the water to obtain an air-entraining agent solution;
[0018] S3. Add polystyrene foam particles, foam stabilizer, remaining water and air entraining agent solution to the first mixture, then add polypropylene fiber, stir evenly to obtain ultra-low carbon thermal insulation mortar.
[0019] Furthermore, in S1 and S2, the stirring speed of the stirring process is 60-90 rpm; in S3, the stirring speed of the stirring process is 120-150 rpm.
[0020] Furthermore, in S2, the mass ratio of the air entraining agent to water is 1 / 20-1 / 30.
[0021] Furthermore, the prepared mortar has a compressive strength of not less than 0.5 MPa, a thermal conductivity of not more than 0.070 W (m·K), and a dry density of not more than 350 kg / m 3 , meeting the requirements of Type I mortar in GB / T 20473-2021 "Building Thermal Insulation Mortar".
[0022] Furthermore, the transportation and use of the prepared mortar are the same as those of conventional mortar. The above-mentioned proportion of recycled concrete powder is for reference only and shall be determined according to the performance requirements of the actual situation during the specific design.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] (1) The present invention prepares a lightweight, high-thermal insulation functional mortar by combining the use of polystyrene foam particles with carbonization curing, and ensures the anti-cracking performance of the mortar by adding polypropylene fibers.
[0025] (2) The present invention also uses recycled concrete powder to replace part of cement clinker, thereby reducing the use of cement clinker and reducing carbon emissions from mortar production. At the same time, it alleviates the pressure on the disposal of construction solid waste, thereby achieving the purpose of saving resources and protecting the environment.
[0026] (3) Based on the porosity of the thermal insulation mortar and the carbon sequestration potential of recycled concrete powder, curing it in a high concentration CO2 environment can effectively improve the strength of the thermal insulation mortar soil and fully exert the carbon sequestration effect of cement-based materials.
[0027] (4) The present invention can recycle construction solid waste to prepare a new type of thermal insulation mortar with excellent performance, and has a relatively broad application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the process of preparing the ultra-low carbon thermal insulation mortar of the present invention. DETAILED DESCRIPTION
[0029] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0030] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. If no specific conditions are specified, the conventional conditions or the conditions recommended by the manufacturer shall be followed. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0031] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0032] With the rapid development of industrialization and urbanization, energy consumption and solid waste generation have come along with it. Among the main solid wastes in my country, general industrial solid waste has the largest generation. In addition, the amount of construction waste in my country has accounted for 30% to 40% of the total urban waste. Although there are many methods for solid waste treatment at present, such as sanitary landfill, incineration, composting, etc. However, these methods will not only occupy a large amount of land and cost a lot of construction funds, but also cause environmental pollution problems during the transportation and stacking process. In the process of urbanization, building solid waste has affected the environment on which human beings depend for survival. At present, the utilization of solid waste is relatively small, and the domestic utilization rate is less than 10%. If the rich components in solid waste can be comprehensively utilized, it will create huge economic and environmental benefits.
[0033] The urbanization process has produced a large amount of waste concrete. In particular, recycled concrete powder with a particle size of less than 75μm is one of its resource products. Recycled concrete powder has been proven to have a certain volcanic ash reaction and can be used as an auxiliary cementitious material to reduce the use of cement clinker. Due to the large amount of calcium materials contained, recycled concrete powder also has great carbon sequestration potential. At the same time, through carbonization curing thermal insulation mortar, CO2 can react with cement hydration products in the pore fluid, and finally generate calcium carbonate on the mortar surface to fill the pores, thereby improving the mechanical properties and impermeability of the mortar.
[0034] In summary, based on the traditional polystyrene thermal insulation mortar technology, the present invention further incorporates polypropylene fibers to improve its crack resistance, uses recycled concrete powder to replace part of the cement clinker, and adopts carbonization curing technology to improve its anti-permeability and reduce its carbon emissions. Thus, a new thermal insulation mortar with an extremely low carbon footprint is prepared.
[0035] like Figure 1 As shown, a method for preparing ultra-low carbon thermal insulation mortar comprises the following steps:
[0036] Step 1: Recycled concrete powder processing:
[0037] Select recycled aggregate factory production, apparent density not more than 2700kg / m 3 Unmodified recycled concrete powder. The large aggregate with a particle size greater than 75μm is screened out by a sorting machine, and excess inorganic impurities are removed, and then sent to a dryer set at a temperature of 105℃ for continuous drying for 24 hours before use.
[0038] Step 2: Screening of polystyrene foam particles:
[0039] The polystyrene foam particles are graded using a screening test. The screening test uses a set of standard sieves with apertures (net size) of 4.75mm, 2.36mm, 1.18mm, 0.60mm, 0.30mm and 0.15mm to sieve 500g of absolute dry polystyrene foam from coarse to fine in sequence and weigh the sieve residues remaining on each sieve, and calculate the individual sieve residues a1, a2, a3, a4, a5, a6 (the percentage of the sieve residue on each sieve to the total sand sample) and the cumulative sieve residues A1, A2, A3, A4, A5, A6. And calculate the fineness modulus as follows:
[0040]
[0041] According to the fineness modulus, polystyrene foam particles can be divided into coarse particle size (M x =3.7-3.1), medium particle size (M x =3.0-2.3), fine particle size (M x =2.3-1.6). For polystyrene foam particles with a fineness modulus within the range of 1.6 to 3.7, the particle gradation shall meet the requirements of any gradation in Table 1. Except for 4.75mm and 0.60mm, the remaining sieve residues are allowed to exceed by no more than 5%.
[0042] Table 1 Requirements for sieve residue of polystyrene foam particles with different gradations
[0043]
[0044] Step 3: Design of mortar mix ratio applicability:
[0045] According to the different needs and basic performance requirements of the insulation mortar usage scenarios, the cementitious material should consider using 50% recycled micro powder and 50% ordinary cement when designing the mix ratio;
[0046] The raw materials weighed mainly include: ordinary Portland cement, recycled micropowder, polystyrene foam particles, air entraining agent, water reducing agent and water; the amounts of raw materials weighed (in parts by mass) are: 400-700 parts of ordinary Portland cement, 300-600 parts of recycled concrete powder, 600-800 parts of water, 90-125 parts of polystyrene foam particles, 20-25 parts of polypropylene fibers, 1-2 parts of air entraining agent, and 1-2 parts of foam stabilizer.
[0047] Step 4: Preparation of ultra-low carbon thermal insulation mortar:
[0048] Prioritize mixing the cementitious material with an appropriate amount of mixing water, and prepare the air entraining agent solution for use. After mixing evenly, add the remaining materials and continue mixing with a high-speed mixer. The method of adding recycled concrete powder and polystyrene foam particles is the same as the conventional mortar preparation method.
[0049] Step 5: Mortar carbonization curing
[0050] The prepared foamed mortar molding specimens are cured in a standard curing room for 1 day and then demolded. The demoulded specimens are then placed in a carbonization chamber with a CO2 concentration of 20%, a temperature of 25±3°C, and a relative humidity of 70±5% for carbonization curing for 7 days or more.
[0051] This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0052] Comparative Example 1 :
[0053] A new type of thermal insulation mortar without recycled concrete powder and conventional curing comprises the following steps:
[0054] 1) Use unmodified recycled concrete powder produced by recycled aggregate factory, with apparent density not more than 2700kg / m 3 , use a sorting machine to screen out large aggregates with a particle size greater than 75μm, remove excess inorganic impurities, and send them to a dryer set at 105℃ for continuous drying for 24 hours before use;
[0055] 2) Use 4.75mm and 0.15mm mesh sieves in the standard sieve set to screen out polystyrene foam particles larger than 4.75mm and smaller than 0.15mm, and ensure that the gradation of the particles is continuous. After cleaning to remove impurities, dry them and place them in a ventilated place indoors for 48 hours for use;
[0056] 3) Select 1000 parts of ordinary Portland cement and 375 parts of water, add them into the mixer in sequence, and stir at a low speed of 60r / min for 2 minutes until the above components are evenly mixed;
[0057] 4) Select 1 part of air-entraining agent and 25 parts of water and add them into a container. Stir at a low speed of 60r / min for 2 minutes until the above components are evenly mixed to obtain an air-entraining agent solution for use;
[0058] 5) Slowly add the prepared air entraining agent solution, 105 parts of dried polystyrene foam particles, 1 part of foam stabilizer and 350 parts of water into the mixer, and gradually add 20 parts of loose polypropylene fibers, and stir at a high speed of 120r / min for 2 minutes until all the materials are evenly mixed;
[0059] 6) The prepared foamed mortar molded sample was cured in a standard curing room for 1 day and then demolded, and then the demolded sample was placed in a standard curing room for further curing for 7 days to obtain an insulating mortar without recycled concrete powder and with ordinary curing.
[0060] Example 1 :
[0061] See also Figure 1 , a new type of thermal insulation mortar containing 30% recycled concrete powder and carbonization curing for 7 days, comprising the following steps:
[0062] 1) Use unmodified recycled concrete powder produced by recycled aggregate factory, with apparent density not more than 2700kg / m 3 , use a sorting machine to screen out large aggregates with a particle size greater than 75μm, remove excess inorganic impurities, and send them to a dryer set at 105℃ for continuous drying for 24 hours before use;
[0063] 2) Use 4.75mm and 0.15mm mesh sieves in the standard sieve set to screen out polystyrene foam particles larger than 4.75mm and smaller than 0.15mm, and ensure that the gradation of the particles is continuous. After cleaning to remove impurities, dry them and place them in a ventilated place indoors for 48 hours for use;
[0064] 3) Select 700 parts of ordinary Portland cement, 300 parts of recycled concrete powder and 375 parts of water, add them into the mixer in sequence, and stir at a low speed of 60r / min for 2 minutes until the above components are evenly mixed;
[0065] 4) Select 1 part of air-entraining agent and 25 parts of water and add them into a container. Stir at a low speed of 60r / min for 2 minutes until the above components are evenly mixed to obtain an air-entraining agent solution for use;
[0066] 5) Slowly add the prepared air entraining agent solution, 105 parts of dried polystyrene foam particles, 1 part of foam stabilizer and 350 parts of water into the mixer, and gradually add 20 parts of loose polypropylene fibers, and stir at a high speed of 120r / min for 2 minutes until all the materials are evenly mixed;
[0067] 6) The prepared foamed mortar molded specimens were cured in a standard curing room for 1 day and then demolded. The demolded specimens were then placed in a carbonization chamber with a CO2 concentration of 20%, a temperature of 25±3°C, and a relative humidity of 70±5% for carbonization curing for 7 days to obtain a new thermal insulation mortar containing 30% recycled concrete powder and carbonization curing for 7 days.
[0068] Example 2 :
[0069] See also Figure 1 , a new type of thermal insulation mortar containing 50% recycled concrete powder and carbonization curing for 3 days, comprising the following steps:
[0070] 1) Use unmodified recycled concrete powder produced by recycled aggregate factory, with apparent density not more than 2700kg / m 3 , use a sorting machine to screen out large aggregates with a particle size greater than 75μm, remove excess inorganic impurities, and send them to a dryer set at 105℃ for continuous drying for 24 hours before use;
[0071] 2) Use 4.75mm and 0.15mm mesh sieves in the standard sieve set to screen out polystyrene foam particles larger than 4.75mm and smaller than 0.15mm, and ensure that the gradation of the particles is continuous. After cleaning to remove impurities, dry them and place them in a ventilated place indoors for 48 hours for use;
[0072] 3) Select 500 parts of ordinary Portland cement, 500 parts of recycled concrete powder and 375 parts of water, add them into the mixer in sequence, and stir at a low speed of 60r / min for 2 minutes until the above components are evenly mixed;
[0073] 4) Select 1 part of air-entraining agent and 25 parts of water and add them into a container. Stir at a low speed of 60r / min for 2 minutes until the above components are evenly mixed to obtain an air-entraining agent solution for use;
[0074] 5) Slowly add the prepared air entraining agent solution, 105 parts of dried polystyrene foam particles, 1 part of foam stabilizer and 350 parts of water into the mixer, and gradually add 20 parts of loose polypropylene fibers, and stir at a high speed of 120r / min for 2 minutes until all the materials are evenly mixed;
[0075] 6) The prepared foamed mortar molded specimens were cured in a standard curing room for 1 day and then demolded. The demolded specimens were then placed in a carbonization chamber with a CO2 concentration of 20%, a temperature of 25±3°C, and a relative humidity of 70±5% for carbonization curing for 3 days to obtain a new thermal insulation mortar containing 50% recycled concrete powder and carbonization curing for 3 days.
[0076] Example 3 :
[0077] See also Figure 1, a new type of thermal insulation mortar containing 50% recycled concrete powder and carbonization curing for 7 days, comprising the following steps:
[0078] 1) Use unmodified recycled concrete powder produced by recycled aggregate factory, with apparent density not more than 2700kg / m 3 , use a sorting machine to screen out large aggregates with a particle size greater than 75μm, remove excess inorganic impurities, and send them to a dryer set at 105℃ for continuous drying for 24 hours before use;
[0079] 2) Use 4.75mm and 0.15mm mesh sieves in the standard sieve set to screen out polystyrene foam particles larger than 4.75mm and smaller than 0.15mm, and ensure that the gradation of the particles is continuous. After cleaning to remove impurities, dry them and place them in a ventilated place indoors for 48 hours for use;
[0080] 3) Select 500 parts of ordinary Portland cement, 500 parts of recycled concrete powder and 375 parts of water, add them into the mixer in sequence, and stir at a low speed of 60r / min for 2 minutes until the above components are evenly mixed;
[0081] 4) Select 1 part of air-entraining agent and 25 parts of water and add them into a container. Stir at a low speed of 60r / min for 2 minutes until the above components are evenly mixed to obtain an air-entraining agent solution for use;
[0082] 5) Slowly add the prepared air entraining agent solution, 105 parts of dried polystyrene foam particles, 1 part of foam stabilizer and 350 parts of water into the mixer, and gradually add 20 parts of loose polypropylene fibers, and stir at a high speed of 120r / min for 2 minutes until all the materials are evenly mixed;
[0083] 6) The prepared foamed mortar molded specimens were cured in a standard curing room for 1 day and then demolded. The demolded specimens were then placed in a carbonization chamber with a CO2 concentration of 20%, a temperature of 25±3°C, and a relative humidity of 70±5% for carbonization curing for 7 days to obtain a new thermal insulation mortar containing 50% recycled concrete powder and carbonized for 7 days.
[0084] The above comparative example 1 and examples 1-3 respectively prepared thermal insulation mortars without recycled concrete powder and conventional curing, new thermal insulation mortars containing 30% recycled concrete powder and carbonization curing for 7 days, new thermal insulation mortars containing 50% recycled concrete powder and carbonization curing for 3 days, and new thermal insulation mortars containing 50% recycled concrete powder and carbonization curing for 7 days. In particular, the mechanical properties and thermal insulation properties of the above examples were respectively carried out in accordance with the requirements of GB / T 5486-2008 "Test methods for inorganic rigid thermal insulation products" and GB / T10294-2008 "Determination of steady-state thermal resistance and related properties of thermal insulation materials". The test results are shown in Table 2. It can be seen that compared with Example 1 (control group), when recycled concrete powder is used to replace 50% of the cement clinker and carbonization curing is performed for 7 days (minimizing carbon emissions), the CO2 emissions in the production process of the ultra-low carbon thermal insulation mortar are only 46.7% of that of the traditional mortar. The ultra-low carbon thermal insulation mortar also has comparable mechanical properties and better functionality, meeting the requirements of GB / T20473-2021 "Building Thermal Insulation Mortar".
[0085] Table 2 Comparison of mortar properties prepared in Comparative Example 1 and Examples 1-3
[0086]
[0087]
[0088] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. An ultra-low carbon thermal insulation mortar, characterized in that: The composition comprises the following components in parts by weight:
2. The ultra-low carbon thermal insulation mortar according to claim 1, characterized in that: The ordinary Portland cement is PO 42.5 grade ordinary Portland cement.
3. The ultra-low carbon thermal insulation mortar according to claim 1, characterized in that: The regenerated micro powder is regenerated concrete powder.
4. The ultra-low carbon thermal insulation mortar according to claim 1, characterized in that: The polystyrene foam particles are formed by mixing polystyrene foam particles of 0.5-1 mm, polystyrene foam particles of 1-2 mm and polystyrene foam particles of 2-5 mm of equal mass.
5. The ultra-low carbon thermal insulation mortar according to claim 1, characterized in that: The polypropylene fiber has an aspect ratio of 333 and a tensile strength of 400-500 MPa.
6. The ultra-low carbon thermal insulation mortar according to claim 1, characterized in that: The air entraining agent is one or more of industrial α-sodium sulfonate, sodium alcohol ether sulfate or sodium dodecyl sulfate.
7. The ultra-low carbon thermal insulation mortar according to claim 1, characterized in that: The foam stabilizer is one or more of hydroxypropyl methylcellulose, calcium stearate or tea saponin.
8. The method for preparing the ultra-low carbon thermal insulation mortar according to any one of claims 1 to 7, characterized in that: The steps include: S1. Mixing ordinary Portland cement, recycled concrete powder and part of water, stirring evenly to obtain a first mixture; S2, stirring the air-entraining agent and part of the water to obtain an air-entraining agent solution; S3. Add polystyrene foam particles, foam stabilizer, remaining water and air entraining agent solution to the first mixture, then add polypropylene fiber, stir evenly to obtain ultra-low carbon thermal insulation mortar.
9. The method for preparing an ultra-low carbon thermal insulation mortar according to claim 8, characterized in that: In S1 and S2, the stirring speed of the stirring process is 60-90 rpm; in S3, the stirring speed of the stirring process is 120-150 rpm.
10. The method for preparing an ultra-low carbon thermal insulation mortar according to claim 8, characterized in that: In S2, the mass ratio of the air entraining agent to water is 1 / 20-1 / 30.
Citation Information
Patent Citations
Mortar for heat preservation and thermal insulation of building outer wall
CN101182166A
Polyphenylene granular thermal-insulation mortar
CN103242014A
Low-carbon cement mortar and preparation method thereof
CN118405886A