Anti-aging polymer cement waterproof coating and preparation method thereof
By using specific ratio powder and liquid materials in polymer cement waterproof coatings, combining UV-proof and crack-resistant materials, the problems of polymer cement waterproof coatings aging and film cracking under light are solved, achieving more lasting and stable waterproof performance.
Patent Information
- Application Number
- CN202411154986.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polymer cement waterproof coatings are prone to aging under long-term light, ultraviolet rays cause polymer chains to break, waterproof performance decreases, and large thickness during construction, and the coating film layer is prone to cracking.
Using a combination of powder and liquid materials, including silicate cement, heavy calcium, gypsum, fillers, tannins, bactericides, UV-proof materials and crack-resistant materials, through the intersection of powder and modified acrylate emulsion The combination reaction increases the density of the waterproof film layer, and reflects the ultraviolet rays through the ultraviolet-proof material, and reduces the cracking of the film layer by combining the cracking-resistant material.
It improves the UV resistance ability of waterproof coatings, reduces cracking of the coating film layer, and ensures the long-lasting stability and waterproof performance of the waterproof layer.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer cement waterproof coating preparation, in particular to an anti-aging polymer cement waterproof coating and a preparation method thereof. Background Art
[0002] Polymer cement waterproof coating is a two-component water-based waterproof coating made of polymer emulsion and cement as the main raw materials, with fillers and other additives added. It is cured into a film through water volatilization and cement hydration reaction, referred to as JS waterproof coating. JS waterproof coating can be directly constructed on a wet or dry base, has good adhesion with mortar and concrete, and has good anti-seepage performance, so it has been widely used in building waterproofing projects in recent years; Existing polymer cement waterproof coatings cannot withstand long-term sunlight. The ultraviolet rays in the sun will cause the polymer chains to break, the coating film to age and degrade, and the waterproof performance will decrease. Therefore, polymer cement waterproof coatings are mostly used indoors in places that are not exposed to sunlight. However, in actual applications, due to reasons such as construction schedule, the waterproof layer of polymer cement waterproof coatings is not covered and protected in time after application, but is left exposed. At the same time, during the construction and coating, the polymer cement waterproof coating is prone to cracking during the film-forming process due to its large thickness.
[0003] Therefore, the present invention provides an anti-aging polymer cement waterproof coating and a preparation method thereof to solve the above-mentioned problems. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides an anti-aging polymer cement waterproof coating and a preparation method thereof, which has high refractive index and improves UV resistance; improves the density of the waterproof film layer, reduces cracking of the coating film layer, ensures the long-term stability of the waterproof layer, and ensures that product performance can be maintained for a long time, thereby solving the problem of cracking of the coating film layer due to its large thickness.
[0005] To achieve the above object, the present invention provides the following technical solution: an anti-aging polymer cement waterproof coating, composed of powder and liquid, the mixing ratio of the powder and the liquid is (1-1.5):1, including the following raw materials in proportion by weight: Powder: 100-120 parts of Portland cement, 50-120 parts of heavy calcium, 10-40 parts of gypsum, 10-20 parts of filler, 10-15 parts of tannic acid, 1-20 parts of fungicide, 1-20 parts of water reducer, 10-30 parts of UV protection material, 10-20 parts of anti-cracking material.
[0006] Liquid material: 100-200 parts of polymer emulsion, 10-35 parts of additives, 10-120 parts of water.
[0007] Preferably, the anti-ultraviolet material is made by mixing white cement, mica powder and titanium dioxide in a ratio of (5-10):1:2; and the anti-cracking material is made by mixing polymer hollow microspheres and carbon fibers in a ratio of (2-3):1.
[0008] Preferably, the water reducer is at least one of a naphthalene-based water reducer, a polycarboxylic acid water reducer and a melamine water reducer, and the filler is made by mixing quartz sand and quartz powder in a ratio of 1:2.
[0009] Preferably, the polymer emulsion is a modified acrylic emulsion, and the modified acrylic emulsion is prepared by reacting methyl acrylate, butyl acrylate, and alkenyl-containing epoxy resin in a mass ratio of 1: (1-2): 1.
[0010] Preferably, the additives include a dispersant, a nonionic polyurethane thickener, a defoaming agent, and a preservative.
[0011] Preferably, the dispersant is at least one of polycarboxylic acid sodium salt and polyacrylate ammonium salt.
[0012] Preferably, the defoamer is at least one of a polyether defoamer, a silicone defoamer and a mineral oil defoamer.
[0013] Another technical problem to be solved by the present invention is to provide a method for preparing an anti-aging polymer cement waterproof coating, comprising the following steps: Step 1: fully mix white cement, mica powder and titanium dioxide according to a predetermined ratio to prepare an anti-ultraviolet material; At the same time, the polymer hollow microspheres and the carbon fibers are fully mixed in a determined ratio to prepare a crack-resistant material; Step 2: Prepare powder: Mix silicate cement, heavy calcium and gypsum in proportion and evenly prepare material 1; Step 3: fully stir tannic acid, UV protection material and anti-cracking material, add filler consisting of quartz sand and quartz powder during the stirring process, stir evenly to obtain the second preparation and evenly divide it into 2-3 portions; Step 4: Then add the fungicide and water reducer into the preparation 1 and stir them thoroughly for 10-30 minutes. Then take a single portion of the preparation 2 and pour it into the preparation 1 at intervals. The addition intervals are the same, and finally a powder is obtained. Step 5: Prepare liquid material: mix the polymer emulsion and water evenly, then add additives, and mix evenly to obtain liquid material; Step 6: When using, fully mix the prepared powder and liquid, and let it stand for 1-3 minutes to obtain the finished polymer cement waterproof coating.
[0014] Compared with the prior art, the present invention provides an anti-aging polymer cement waterproof coating and a preparation method thereof, which has the following beneficial effects: 1. The anti-aging polymer cement waterproof coating and its preparation method can react and cross-link with the active groups such as epoxy groups on the modified acrylic emulsion through the materials in the powder, so that the modified acrylic emulsion, cement hydration products and fillers are more tightly combined, the density of the waterproof film layer is improved, the cracking of the coating film layer is reduced, and the long-term stability of the waterproof layer is ensured.
[0015] 2. The anti-aging polymer cement waterproof coating and its preparation method, by adding anti-ultraviolet material, can reflect and refract ultraviolet rays by utilizing the high refractive index of the material, thereby reducing the influence of light on the coating film and improving the durability of the waterproof layer. DETAILED DESCRIPTION
[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example
[0017] An anti-aging polymer cement waterproof coating, composed of powder and liquid, the mixing ratio of the powder and liquid is 1:1, including the following raw materials in proportion by weight: Powder: 100 parts of Portland cement, 50 parts of heavy calcium, 10 parts of gypsum, 10 parts of filler, 10 parts of tannic acid, 1 part of fungicide, 1 part of water reducing agent, 10 parts of UV protection material, 10 parts of anti-cracking material; The anti-ultraviolet material is made of white cement, mica powder and titanium dioxide in a ratio of 5:1:2; the anti-cracking material is made of polymer hollow microspheres and carbon fiber in a ratio of 2:1; The water reducer is a naphthalene-based water reducer, and the filler is made by mixing quartz sand and quartz powder in a ratio of 1:2.
[0018] Liquid material: 100 parts of polymer emulsion, 10 parts of additives, 10 parts of water; The polymer emulsion is a modified acrylic emulsion, which is prepared by reacting methyl acrylate, butyl acrylate and alkenyl-containing epoxy resin in a mass ratio of 1:1:1. Additives include dispersants, nonionic polyurethane thickeners, defoamers, and preservatives; The dispersant is polycarboxylic acid sodium salt, and the defoamer is a polyether defoamer.
[0019] A method for preparing an anti-aging polymer cement waterproof coating comprises the following steps: Step 1: fully mix white cement, mica powder and titanium dioxide according to a predetermined ratio to prepare an anti-ultraviolet material; At the same time, the polymer hollow microspheres and the carbon fibers are fully mixed in a determined ratio to prepare a crack-resistant material; Step 2: Prepare powder: Mix silicate cement, heavy calcium and gypsum in proportion and evenly prepare material 1; Step 3: fully stir tannic acid, UV protection material and anti-cracking material, add filler consisting of quartz sand and quartz powder during the stirring process, stir evenly to obtain the second preparation and divide it evenly into 2 parts; Step 4: Then add the fungicide and water reducer into the preparation 1 and stir them thoroughly for 10 minutes. Then take a single portion of the preparation 2 and pour it into the preparation 1 at intervals. The addition intervals are the same, and finally a powder is obtained. Step 5: Prepare liquid material: mix the polymer emulsion and water evenly, then add additives, and mix evenly to obtain liquid material; Step 6: When using, fully mix the prepared powder and liquid, and let it stand for 1 minute to obtain the finished polymer cement waterproof coating. Example
[0020] An anti-aging polymer cement waterproof coating, composed of powder and liquid, the mixing ratio of the powder and liquid is 1.5:1, including the following raw materials in proportion by weight: Powder: 120 parts of Portland cement, 120 parts of heavy calcium, 40 parts of gypsum, 20 parts of filler, 15 parts of tannic acid, 20 parts of fungicide, 20 parts of water reducer, 30 parts of UV protection material, 20 parts of anti-cracking material; The anti-ultraviolet material is made of white cement, mica powder and titanium dioxide in a ratio of 10:1:2; the anti-cracking material is made of polymer hollow microspheres and carbon fiber in a ratio of 3:1; The water reducing agent is melamine water reducing agent, and the filler is made of quartz sand and quartz powder mixed in a ratio of 1:2.
[0021] Liquid material: 200 parts of polymer emulsion, 35 parts of additives, 120 parts of water; The polymer emulsion is a modified acrylic emulsion, which is prepared by reacting methyl acrylate, butyl acrylate and alkenyl-containing epoxy resin in a mass ratio of 1:2:1. Additives include dispersants, nonionic polyurethane thickeners, defoamers, and preservatives; The dispersant is ammonium polyacrylate, and the defoamer is an organosilicon defoamer.
[0022] A method for preparing an anti-aging polymer cement waterproof coating comprises the following steps: Step 1: fully mix white cement, mica powder and titanium dioxide according to a predetermined ratio to prepare an anti-ultraviolet material; At the same time, the polymer hollow microspheres and the carbon fibers are fully mixed in a determined ratio to prepare a crack-resistant material; Step 2: Prepare powder: Mix silicate cement, heavy calcium and gypsum in proportion and evenly prepare material 1; Step 3: fully stir tannic acid, UV protection material and anti-cracking material, add filler consisting of quartz sand and quartz powder during the stirring process, stir evenly to obtain the second preparation and evenly divide it into 3 parts; Step 4: Then add the fungicide and water reducer into the preparation 1 and stir them thoroughly for 30 minutes. Then take a single portion of the preparation 2 and pour it into the preparation 1 at intervals. The addition intervals are the same, and finally a powder is obtained. Step 5: Prepare liquid material: mix the polymer emulsion and water evenly, then add additives, and mix evenly to obtain liquid material; Step 6: When using, fully mix the prepared powder and liquid, and let it stand for 3 minutes to obtain the finished polymer cement waterproof coating. Example
[0023] An anti-aging polymer cement waterproof coating is composed of powder and liquid, the mixing ratio of the powder and liquid is 1.2:1, and includes the following raw materials in proportion by weight: Powder: 100 parts of Portland cement, 100 parts of heavy calcium, 10 parts of gypsum, 10 parts of filler, 13 parts of tannic acid, 13 parts of fungicide, 13 parts of water reducer, 23 parts of UV protection material, 13 parts of anti-cracking material; The anti-ultraviolet material is made of white cement, mica powder and titanium dioxide in a ratio of 7:1:2; the anti-cracking material is made of polymer hollow microspheres and carbon fiber in a ratio of 2.5:1; The water reducer is a mixture of naphthalene water reducer, polycarboxylic acid water reducer and melamine water reducer, and the filler is made of quartz sand and quartz powder mixed in a ratio of 1:2.
[0024] Liquid material: 135 parts of polymer emulsion, 11 parts of additives, 55 parts of water; The polymer emulsion is a modified acrylic emulsion, which is prepared by reacting methyl acrylate, butyl acrylate and alkenyl-containing epoxy resin in a mass ratio of 1:1:1. Additives include dispersants, nonionic polyurethane thickeners, defoamers, and preservatives; The dispersant is sodium polycarboxylate, and the defoamer is mineral oil defoamer.
[0025] A method for preparing an anti-aging polymer cement waterproof coating comprises the following steps: Step 1: fully mix white cement, mica powder and titanium dioxide according to a predetermined ratio to prepare an anti-ultraviolet material; At the same time, the polymer hollow microspheres and the carbon fibers are fully mixed in a determined ratio to prepare a crack-resistant material; Step 2: Prepare powder: Mix silicate cement, heavy calcium and gypsum in proportion and evenly prepare material 1; Step 3: fully stir tannic acid, UV protection material and anti-cracking material, add filler consisting of quartz sand and quartz powder during the stirring process, stir evenly to obtain the second preparation and evenly divide it into 3 parts; Step 4: Then add the fungicide and water reducer into the preparation 1 and stir them thoroughly for 30 minutes. Then take a single portion of the preparation 2 and pour it into the preparation 1 at intervals. The addition intervals are the same, and finally a powder is obtained. Step 5: Prepare liquid material: mix the polymer emulsion and water evenly, then add additives, and mix evenly to obtain liquid material; Step 6: When using, fully mix the prepared powder and liquid, and let it stand for 3 minutes to obtain the finished polymer cement waterproof coating. Example
[0026] An anti-aging polymer cement waterproof coating, composed of powder and liquid, the mixing ratio of the powder and liquid is 1:1, including the following raw materials in proportion by weight: Powder: 100 parts of Portland cement, 50 parts of heavy calcium, 10 parts of gypsum, 10 parts of filler, 10 parts of tannic acid, 1 part of fungicide, 1 part of water reducing agent, 10 parts of UV protection material, 10 parts of anti-cracking material; The anti-ultraviolet material is made of white cement, mica powder and titanium dioxide in a ratio of 5:1:2; the anti-cracking material is made of polymer hollow microspheres and carbon fiber in a ratio of 2:1; The water reducer is a naphthalene-based water reducer, and the filler is made by mixing quartz sand and quartz powder in a ratio of 1:2.
[0027] Liquid material: 150 parts of polymer emulsion, 20 parts of additives, 100 parts of water; The polymer emulsion is a modified acrylic emulsion, which is prepared by reacting methyl acrylate, butyl acrylate and alkenyl-containing epoxy resin in a mass ratio of 1:2:1. Additives include dispersants, nonionic polyurethane thickeners, defoamers, and preservatives; The dispersant is a mixture of polycarboxylic acid sodium salt and polyacrylic acid ammonium salt, and the defoamer is a mixture of polyether defoamer, silicone defoamer and mineral oil defoamer.
[0028] A method for preparing an anti-aging polymer cement waterproof coating comprises the following steps: Step 1: fully mix white cement, mica powder and titanium dioxide according to a predetermined ratio to prepare an anti-ultraviolet material; At the same time, the polymer hollow microspheres and the carbon fibers are fully mixed in a determined ratio to prepare a crack-resistant material; Step 2: Prepare powder: Mix silicate cement, heavy calcium and gypsum in proportion and evenly prepare material 1; Step 3: fully stir tannic acid, UV protection material and anti-cracking material, add filler consisting of quartz sand and quartz powder during the stirring process, stir evenly to obtain the second preparation and divide it evenly into 2 parts; Step 4: Then add the fungicide and water reducer into the preparation 1 and stir them thoroughly for 10 minutes. Then take a single portion of the preparation 2 and pour it into the preparation 1 at intervals. The addition intervals are the same, and finally a powder is obtained. Step 5: Prepare liquid material: mix the polymer emulsion and water evenly, then add additives, and mix evenly to obtain liquid material; Step 6: When using, fully mix the prepared powder and liquid, and let it stand for 1 minute to obtain the finished polymer cement waterproof coating.
[0029] The beneficial effects of the present invention are as follows: the anti-aging polymer cement waterproof coating and the preparation method thereof can react and cross-link with active groups such as epoxy groups on the modified acrylic ester emulsion through the materials in the powder, so that the modified acrylic ester emulsion, cement hydration products and fillers are more tightly combined, the density of the waterproof film layer is improved, the cracking of the coating film layer is reduced, and the long-term stability of the waterproof layer is ensured. By adding anti-ultraviolet materials, the high refractive index of the materials can be used to reflect and refract ultraviolet rays, reduce the influence of light on the coating film, and improve the durability of the waterproof layer.
[0030] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An anti-aging polymer cement waterproof coating, It is characterized in that It is composed of powder and liquid, the mixing ratio of powder and liquid is (1-1.5):1, including the following raw materials in proportion by weight: Powder: 100-120 parts of Portland cement, 50-120 parts of heavy calcium, 10-40 parts of gypsum, 10-20 parts of filler, 10-15 parts of tannic acid, 1-20 parts of fungicide, 1-20 parts of water reducing agent, 10-30 parts of UV protection material, 10-20 parts of anti-cracking material; Liquid material: 100-200 parts of polymer emulsion, 10-35 parts of additives, 10-120 parts of water.
2. An anti-aging polymer cement waterproof coating according to claim 1, It is characterized in that The anti-ultraviolet material is prepared by mixing white cement, mica powder and titanium dioxide in a ratio of (5-10):1:2; the anti-cracking material is prepared by mixing polymer hollow microspheres and carbon fibers in a ratio of (2-3):
1.
3. The anti-aging polymer cement waterproof coating according to claim 1, It is characterized in that The water reducer is at least one of a naphthalene-based water reducer, a polycarboxylic acid water reducer and a melamine water reducer, and the filler is prepared by mixing quartz sand and quartz powder in a ratio of 1:
2.
4. The anti-aging polymer cement waterproof coating according to claim 1, It is characterized in that The polymer emulsion is a modified acrylic emulsion, which is prepared by reacting methyl acrylate, butyl acrylate and alkenyl-containing epoxy resin in a mass ratio of 1: (1-2):
1.
5. The anti-aging polymer cement waterproof coating according to claim 1, It is characterized in that The additives include dispersants, non-ionic polyurethane thickeners, defoamers and preservatives.
6. An anti-aging polymer cement waterproof coating according to claim 5, It is characterized in that The dispersant is at least one of polycarboxylic acid sodium salt and polyacrylic acid ammonium salt.
7. The anti-aging polymer cement waterproof coating according to claim 5, It is characterized in that The defoamer is at least one of a polyether defoamer, a silicone defoamer and a mineral oil defoamer.
8. A method for preparing an anti-aging polymer cement waterproof coating according to any one of claims 1 to 7, It is characterized in that The following steps are involved: Step 1: fully mix white cement, mica powder and titanium dioxide according to a predetermined ratio to prepare an anti-ultraviolet material; At the same time, the polymer hollow microspheres and the carbon fibers are fully mixed in a determined ratio to prepare a crack-resistant material; Step 2: Prepare powder: Mix silicate cement, heavy calcium and gypsum in proportion and evenly prepare material 1; Step 3: fully stir tannic acid, UV protection material and anti-cracking material, add filler consisting of quartz sand and quartz powder during the stirring process, stir evenly to obtain the second preparation and evenly divide it into 2-3 portions; Step 4: Then add the fungicide and water reducer into the preparation 1 and stir them thoroughly for 10-30 minutes. Then take a single portion of the preparation 2 and pour it into the preparation 1 at intervals. The addition intervals are the same, and finally a powder is obtained. Step 5: Prepare liquid material: mix the polymer emulsion and water evenly, then add additives, and mix evenly to obtain liquid material; Step 6: When using, fully mix the prepared powder and liquid, and let it stand for 1-3 minutes to obtain the finished polymer cement waterproof coating.
Citation Information
Cited By
Waterproof coating composition, waterproof coating, and preparation method and application thereof
CN120554904A