Inorganic artificial stone plate and preparation process thereof
By improving the stirring process and using fibers of different lengths, the problem of uneven fiber dispersion in traditional artificial stone slabs is solved, the mechanical properties and durability of the sheets are improved, and the optimal balance between performance and cost is achieved.
Patent Information
- Application Number
- CN202411206696.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
AI Technical Summary
The fibers in traditional artificial stone slabs are difficult to disperse uniformly, resulting in unstable mechanical properties, weak compressive and flexural resistance, poor impact resistance of ball falling and freezing resistance, and high water absorption.
By improving the stirring process and using fibers of different lengths, combined with an optimized water-glue ratio and multi-stage calcium sand filling strategy, we ensure that the fibers are evenly dispersed in the slurry and improve the overall performance of the sheet.
It significantly improves the crack resistance, impact resistance and frost resistance of inorganic artificial stone slabs, reduces water absorption, enhances waterproof performance and durability, and achieves the best balance between performance and cost.
Smart Images

Figure BDA0005019221800000151 
Figure BDA0005019221800000161
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building decoration materials, and in particular to an inorganic artificial stone plate and a preparation process thereof. Background Art
[0002] In the field of building materials, artificial stone, as a high-performance composite material, is widely used in architectural decoration, home decoration and other fields due to its good physical and chemical properties and beautiful appearance. Traditional artificial stone is mainly composed of inorganic cementitious materials (such as cement), fine aggregates (such as sand), coarse aggregates, pigments and various additives. In order to enhance the mechanical properties of artificial stone, the addition of fiber has become an effective means. Fibers can significantly improve the toughness of concrete-based materials and reduce cracking, thereby extending the service life of artificial stone products. However, the application of fibers in artificial stone faces several key technical challenges: the uneven dispersion of fibers in the mixture will lead to unstable performance of artificial stone, especially under low water-cement ratio (the ratio of water to cementitious materials) conditions, the fluidity of aggregates is low, and fibers are easy to agglomerate, which seriously affects the microstructure and macroscopic properties of artificial stone. Although the use of special fibers (such as steel-like fibers) can improve the performance of artificial stone, their high cost limits their large-scale application. At the same time, pretreatment of fibers to improve their dispersibility usually requires additional chemical reagents and processes, which increases production costs and complexity.
[0003] Currently, the industry is trying to solve the above problems by using special fibers and pretreatment technologies. For example, imitation steel fibers are widely used due to their excellent dispersibility and strength, but their high price has become a major bottleneck. Another method is to chemically treat the fiber surface to improve its compatibility and dispersibility with the matrix material, but this also increases production costs and process complexity.
[0004] In summary, although the existing technology has improved the performance of artificial stone to a certain extent, it still needs to be improved in terms of cost control, production efficiency and process simplicity. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention proposes a non-polar artificial stone board and a preparation process thereof, which solves the problem that in the traditional preparation process, the fibers are difficult to be evenly dispersed in the artificial stone matrix, resulting in inconsistent mechanical properties of the board, weak compression and flexural properties, poor falling ball impact resistance and frost resistance, high water absorption and other problems. The present invention improves the stirring process and fibers of different lengths to ensure that the fibers are fully dispersed in the slurry, thereby significantly improving the overall performance of the board.
[0007] (II) Technical solution
[0008] In order to achieve the above object, the main technical solutions adopted by the present invention include:
[0009] In a first aspect, the present application provides an inorganic artificial stone plate, which is formed by beating powder and calcium sand with a particle size of 10 mesh and 20 mesh into slurry under the action of an auxiliary agent, and then adding aggregates to vacuum vibration pressing, wherein the powder includes silicate cement and inorganic pigments, the slurry includes silicate cement, inorganic pigments and calcium sand with a particle size of 10 mesh and 20 mesh, the auxiliary agent includes an active agent, a water reducer and a toughening agent, and the aggregate includes calcium sand with a particle size of 40 mesh, 60 mesh, 80 mesh, 100 mesh, 325 mesh and fiber;
[0010] The artificial stone plate comprises the following components:
[0011] The calcium sand with a particle size of 10 mesh has a mass fraction of 10-20 parts;
[0012] The calcium sand with a particle size of 20 mesh has a mass fraction of 5-10 parts;
[0013] The calcium sand with a particle size of 40 mesh has a mass fraction of 5-8 parts;
[0014] The calcium sand with a particle size of 60 mesh has a mass fraction of 3-4 parts;
[0015] The calcium sand with a particle size of 80 mesh has a mass fraction of 10-15 parts;
[0016] The calcium sand with a particle size of 100 mesh has a mass fraction of 12-17 parts;
[0017] The calcium sand with a particle size of 325 mesh has a mass fraction of 5-7 parts;
[0018] Active agent, the mass fraction thereof is 2-5 parts;
[0019] Inorganic pigment, its mass fraction is 0.1-0.5 parts;
[0020] Fiber, the mass fraction thereof is 0.2-0.6 parts;
[0021] Gel material, 23-37 parts by weight;
[0022] The water-to-gel ratio between water and gel material ranges from 0.15 to 0.20;
[0023] The gel material includes silicate cement, water reducing agent and toughening agent, among which:
[0024] Portland cement, 20-30 parts by mass;
[0025] Water reducing agent, the mass fraction thereof is 1-2 parts;
[0026] Toughening agent, its weight proportion is 2-5 parts.
[0027] In addition, the preparation process also includes water, which is 1-3 parts by weight;
[0028] The board's falling ball impact resistance and frost resistance are significantly enhanced, thanks to the uniform distribution of fibers and the synergistic effect of toughening agents, which enables the board to maintain good stability and durability in extreme environments.
[0029] The board of the present invention has a lower water absorption rate, which is due to the uniform distribution of fibers and the optimized water-to-binder ratio, so that the board structure is denser, effectively resisting water intrusion, and improving the waterproof performance of the board.
[0030] By precisely controlling the mass fraction of each raw material component, the present invention achieves an optimal balance between performance and cost, which not only improves the comprehensive performance of the board but also ensures the economy of production costs.
[0031] The reasonable addition of toughening agents and activators not only enhances the impact resistance and crack resistance of the board, but also promotes the good bonding between the fiber and the matrix material, improving the overall toughness and durability of the board.
[0032] The water-to-gel ratio between water and gel material is strictly controlled between 0.15-0.20, which not only ensures good fluidity of the slurry, but also ensures high strength of the final board, achieving dual optimization of mechanical properties and construction performance.
[0033] Low water-cement ratio is conducive to the formation of a more compact microstructure, which improves the compressive strength, flexural strength and impact resistance of inorganic artificial stone panels. This is because a lower water-cement ratio promotes a more complete cement hydration reaction and forms a denser hardened structure.
[0034] Although the fluidity of the slurry is relatively low under the condition of low water-binder ratio, the fibers can still be evenly dispersed in the slurry through the stirring process of the present invention. This is because the appropriate water-binder ratio ensures good combination of the fibers with the matrix material during the stirring process, avoids the agglomeration of the fibers, and thus improves the overall performance of the board.
[0035] The water-cement ratio controlled within the range of 0.15-0.20 helps to form a structure with fewer pores, reduces the generation of micro cracks, and improves the crack resistance and impermeability of inorganic artificial stone panels. This is of great significance in terms of waterproofing, moisture resistance and long-term durability of buildings.
[0036] Under low water-cement ratio conditions, the freeze-thaw cycle resistance and corrosion resistance of inorganic artificial stone panels are improved due to the denser structure of the hardened body, thus extending the service life of the material.
[0037] Low water-to-binder ratio helps control the water absorption of inorganic artificial stone panels, allowing them to maintain good physical properties in a humid or water-soaked environment. This is especially important for outdoor or high humidity applications.
[0038] Although a low water-to-binder ratio will increase the difficulty of construction, the present invention ensures good construction performance even under low water-to-binder ratio conditions through optimized mixing process and uniform dispersion of fibers, thereby reducing material costs and maintenance costs while ensuring quality.
[0039] Coarse-grained calcium sand includes 10 mesh and 20 mesh. Large-grained calcium sand can fill the larger gaps in the board, play a role in supporting and strengthening the structure, and reduce the shrinkage of the overall material. Coarse-grained calcium sand is usually low-cost, and using more coarse particles can reduce production costs. The coarse particles have a rough surface, which increases the friction of the board and improves the wear resistance.
[0040] Medium-sized calcium sand includes 40 mesh and 60 mesh. Medium-sized particles play a transitional role between coarse particles and fine particles, helping to form a continuous skeleton structure and improve the stability and strength of the board. The appropriate proportion of medium particles helps to reduce microcracks caused by shrinkage and enhance the crack resistance of the board.
[0041] Fine-grained calcium sand includes 80 mesh to 325 mesh. Fine-grained calcium sand can fill smaller gaps, making the board structure more compact and the surface smoother. Fine particles can better combine with resin or other adhesives to enhance the bonding strength of the interface. The addition of fine particles helps to improve the board's impermeability, reduce water penetration, and improve weather resistance and extend service life.
[0042] The comprehensive use of calcium sand of different mesh sizes can achieve multi-level filling of the internal structure of the board, thereby obtaining the best mechanical properties, aesthetics and durability. This multi-level filling strategy improves the overall performance of the board. Different mesh sizes of calcium sand should be mixed in a certain proportion to achieve the best performance balance. For example, too many fine particles will affect the fluidity and processability of the board, while too many coarse particles will lead to uneven density and reduced strength of the board. Therefore, precise control of the mass fraction of calcium sand of each mesh size is the key to manufacturing high-quality inorganic artificial stone boards.
[0043] Too much activator will reduce the strength of the board, because it interferes with the hydration process of cement and affects the formation of hardened body. Insufficient activator cannot fully play its reinforcing role, resulting in reduced strength and durability of the board.
[0044] Too much inorganic pigment will absorb too much water, affect the water-binder ratio, and reduce the strength of the board. Too little inorganic pigment will cause uneven color or different depths, affecting the appearance quality of the board.
[0045] Too much fiber will make the slurry too dense, affect the dispersion of the fiber, and reduce the performance of the board. Too little fiber: Insufficient fiber will weaken the board's crack resistance, impact resistance and frost resistance.
[0046] Too much gel material (Portland cement, water reducer, toughening agent) will increase the cost, and excessive cement will generate too much heat during the curing process, causing volume change and cracking. Too little gel material and insufficient cement will affect the formation of the hardened body, and insufficient water reducer and toughening agent will reduce the fluidity and toughness of the board, affecting the compression and flexural properties.
[0047] The addition of fibers (such as polypropylene fibers, glass fibers, etc.) can significantly improve the crack resistance, impact resistance and frost resistance of artificial stone. When the fibers are evenly dispersed in the matrix formed by calcium sand particles and cementitious materials (such as cement), they can prevent or delay the expansion of cracks at the microscopic level and enhance the overall toughness of the material.
[0048] The different particle sizes of calcium sand (from coarse to fine) provide multi-level filling, forming a continuous skeleton structure. The fibers are embedded in this skeleton and jointly bear the external force, thereby enhancing the compression and flexural properties of the board.
[0049] The presence of water reducer reduces the amount of water required to achieve ideal fluidity, thereby reducing the water-binder ratio, which helps to improve the strength and durability of the hardened body. At the same time, a lower water-binder ratio helps to evenly disperse the fibers in the slurry and avoid fiber agglomeration. Under low water-binder ratio conditions, water reducer can also improve the pumpability and pourability of the slurry, which is particularly important for mixtures containing fibers because the addition of fibers tends to increase the viscosity of the mixture.
[0050] Activators (such as fly ash, silica fume, etc.) can participate in the side reactions of cement hydration to generate more hydration products, which can fill micropores and increase the density of the hardened body. When fibers are added to this denser matrix, the crack resistance and impermeability of the material can be further enhanced. The use of activators can also help reduce the amount of cement, thereby reducing production costs, while maintaining or improving the performance of the board.
[0051] The cement hydration process forms a hard gel structure, and the fiber plays the role of reinforcing tendons in this structure, improving the tensile strength and bending strength of the entire system. When the fiber is closely combined with the cement hydration product, a more complex microstructure can be formed, which can more effectively resist external stress and improve the overall performance of the board.
[0052] Further, the fiber length is 6-10 mm, wherein: the fiber with a length of 6 mm accounts for 60%-70% of the total fiber mass, the fiber with a length of 8 mm accounts for 29.8%-39.6% of the total fiber mass, and the fiber with a length of 10 mm accounts for 0.2%-0.4% of the total fiber mass;
[0053] The fiber is polypropylene fiber or glass fiber.
[0054] 6mm fiber is the main fiber. The length of 6mm fiber is moderate and can be evenly dispersed in the board to form a stable fiber network, which effectively improves the compression and flexural strength of the board. When the board is subjected to stress, the fiber network can disperse the stress and prevent brittle fracture caused by stress concentration. Due to the high distribution density of 6mm fiber, it can effectively prevent the generation and expansion of microcracks, thereby improving the overall crack resistance of the board.
[0055] As auxiliary fibers, 8mm fibers are slightly longer than 6mm fibers, and can form a longer "bridge" inside the board, improving the board's ability to resist external impact, especially in the case of heavy objects falling, which can effectively absorb and disperse the impact energy and enhance the board's resistance to falling ball impact. When subjected to tension, 8mm fibers can provide stronger support to avoid cracks inside the board, thereby improving the tensile strength.
[0056] As a trace fiber, 10mm fiber accounts for a small proportion, but its random distribution in the board can form a special stress dispersion mechanism, especially when the temperature changes, it can relieve the internal stress caused by thermal expansion and contraction, and improve the antifreeze performance of the board. The presence of super-long fibers in the board can prevent the rapid expansion of cracks, while reducing the width and number of cracks, thereby reducing the water penetration and indirectly improving the water absorption rate of the board.
[0057] If the 6mm fiber ratio is too low, the fiber network in the board will become sparse and the crack resistance will be weakened because there is a lack of sufficient short fibers to effectively inhibit the formation and expansion of microcracks. On the contrary, if the 6mm fiber ratio is too high, too many fibers will reduce the fluidity of the slurry, affect the uniform distribution of the fibers, and also reduce the crack resistance.
[0058] As auxiliary fibers, insufficient proportion of 8mm fibers will reduce the stress dispersion inside the board and reduce its ability to resist external impact. Excessive proportion will affect the forming and overall performance of the board because it is more difficult to evenly distribute longer fibers.
[0059] Although the proportion of 10mm fiber is small, it plays an important role in improving the antifreeze performance. Too low a proportion will weaken the board's ability to resist freeze-thaw cycles, while too high a proportion will affect the processing performance and cost of the board.
[0060] In summary, by introducing fibers of different lengths into inorganic artificial stone panels and controlling their respective proportions, the panels' compression and flexural resistance, ball drop impact resistance, frost resistance, and water absorption can be effectively improved. 6mm fibers, as the main fibers, lay the foundation for the basic strength and crack resistance of the panels; 8mm fibers, as auxiliary fibers, enhance impact resistance and tensile strength; and 10mm fibers, as trace fibers, focus on improving frost resistance and further optimizing crack resistance. This multi-level fiber ratio strategy achieves a comprehensive improvement in panel performance and meets the needs of modern architecture for high performance and high durability of materials.
[0061] Furthermore, calcium sand with specifications of 10 mesh and 20 mesh, accounting for 27%-34% of the total calcium sand mass, is added during the beating process to increase friction, and evenly disperse the silicate cement, active agent, inorganic pigment and fiber without causing powder agglomeration and fiber entanglement, thereby increasing the dispersion of aggregate and fiber.
[0062] Furthermore, the toughening agent is at least one of styrene-butadiene emulsion, silicone-acrylic emulsion and pure acrylic emulsion.
[0063] Furthermore, the active agent is at least one of white fly ash, white silica fume and metakaolin.
[0064] Furthermore, the water reducing agent is a polycarboxylic acid water reducing agent.
[0065] In a second aspect, the present invention provides a process for preparing an inorganic artificial stone plate, comprising the following steps:
[0066] S1. Mix silicate cement, active agent, inorganic pigment and calcium sand with specifications of 10 mesh and 20 mesh accounting for 27%-34% of the total calcium sand mass, perform preliminary dry mixing, and stir evenly;
[0067] S2. Add water reducing agent, water and toughening agent to the mixture of step S1, control the water-binder ratio to 0.15-0.20, and stir at different speeds to ensure that all liquids and dry powders are fully mixed to form a uniform slurry;
[0068] S3, adding fibers with a specification of 6 mm-10 mm to the slurry in step S2, wherein the fibers with a length of 6 mm account for 60%-70% of the total fiber mass, the fibers with a length of 8 mm account for 29.8%-39.6% of the total fiber mass, and the fibers with a length of 10 mm account for 0.2%-0.4% of the total fiber mass, and continue stirring to ensure that the fibers are evenly dispersed in the slurry;
[0069] S4, adding the remaining calcium sand aggregate to the slurry in step S3, and stirring again until all the ingredients are completely and evenly mixed to form a mixture with a uniform texture;
[0070] S5, filling the mixed material in step S4 into a mold, and pressing and forming a rough board under vacuum;
[0071] S6. Curing the rough board after being pressed and formed in step S5.
[0072] In step S1, the initial dry mixing of silicate cement, inorganic pigments, and 10-mesh and 20-mesh calcium sand aggregates, which account for 27%-34% of the total calcium sand mass, ensures that these ingredients are evenly distributed before the subsequent addition of water. Dry mixing helps to avoid the aggregation of cement particles and promotes the uniform fusion of pigments and aggregates, thereby forming a consistent color and appearance in the final product. In addition, the initial mixing of coarse-grained calcium sand provides the necessary skeleton structure for the subsequent mixture, which helps to improve the compressive strength and stability of the board. At the same time, the gaps between the coarse particles can reduce moisture retention and help reduce water absorption.
[0073] In step S2, water-reducing agent, water and toughening agent are added to S1, and the water-cement ratio is controlled between 0.15-0.20, which can significantly optimize the fluidity of the slurry while ensuring the strength and density of the hardened body. The use of water-reducing agent reduces the amount of water required, helps to form a denser structure, reduces porosity, thereby improving compression and flexural properties, and reduces water absorption. The addition of toughening agent can improve the toughness of the board, enhance its impact resistance and frost resistance, and make it less likely to crack under external forces or low temperature conditions.
[0074] In step S3, pre-weighed fibers of 6mm-10mm in length are added to the slurry of step S2, with special attention paid to the length distribution ratio of the fibers, which can greatly improve the crack resistance, impact resistance and frost resistance of the board. The uniform distribution of fibers in the slurry can effectively inhibit the formation and expansion of microcracks, increase the toughness of the board, and improve its bending resistance. In addition, the "bridge" effect of the fibers helps to disperse stress and reduce concentrated stress points, thereby improving compressive resistance and resistance to falling ball impact. By controlling the length and ratio of the fibers, water absorption can also be optimized because the evenly dispersed fiber network can reduce the channels for water penetration.
[0075] In step S4, the remaining calcium sand aggregate, including calcium sand of different mesh sizes, is added to the mixture of step S3 to further improve the multi-level filling structure of the board and improve its density and compressive strength. Calcium sand aggregates of different particle sizes can fill voids of different sizes to form a denser structure, reduce water absorption, and improve compression and flexural properties. By controlling the ratio of calcium sand of different mesh sizes, the crack resistance and frost resistance of the board can also be optimized, because fine-grained calcium sand can fill tiny pores and reduce internal stress, while coarse-grained calcium sand provides additional structural support.
[0076] In step S5, the pressing and molding is performed under vacuum, which can remove air, reduce internal bubbles, improve the density of the board, and enhance the compression, bending and frost resistance. The vacuum pressure also helps to distribute the fibers and other components more evenly, ensure the uniformity of the board structure, and reduce water absorption.
[0077] In step S6, proper curing conditions can ensure that the cement is fully hydrated, forming a stable hardened body and improving the strength and durability of the board. Reasonable temperature and humidity control can help reduce cracking, further optimize the compression and flexural properties, improve the frost resistance, and control the water absorption rate to ensure that the board meets the expected performance standards.
[0078] In summary, each step from S1 to S6 is to optimize the comprehensive performance of inorganic artificial stone panels, including key indicators such as compression and flexural resistance, ball impact resistance, frost resistance, and water absorption. Through the preparation process, it can be ensured that the final product not only has excellent physical and mechanical properties, but also meets the requirements of aesthetics, durability, and cost-effectiveness in specific applications.
[0079] Furthermore, in S1, the stirring speed is 45-55 r / min, and the stirring time is 1-2 min; in S2, the stirring speed is first 140-160 r / min, the stirring time is 0.4-0.6 min, and then the stirring speed is 290-310 r / min, and the stirring time is 3-5 min; in S3 and S4, the stirring speeds are both 290-310 r / min, and the stirring time is both 3-5 min.
[0080] Through the optimized mixing process, the fibers are evenly dispersed in the matrix, avoiding fiber agglomeration, significantly improving the consistency of the compressive and flexural strength of the board, and reducing performance fluctuations caused by uneven fiber distribution.
[0081] S1 medium-low speed stirring at 45-55r / min for 1-2 minutes ensures that cement, active agent, sand and inorganic pigment are evenly mixed and avoids agglomeration of dry powder components. This process helps to form a uniform matrix, laying a good foundation for subsequent hydration reactions. A uniform matrix can reduce irregular structures in the board and improve compression, flexural and falling ball impact resistance.
[0082] In S2, the medium speed of 140-160r / min is used for stirring for 0.4-0.6 minutes, which helps to initially disperse the liquid components, and then the high speed of 290-310r / min is used for stirring for 3-5 minutes to ensure that all liquid and dry powder components are fully mixed to form a uniform slurry. This series of stirring operations can improve the fluidity of the slurry, improve the dispersion of fibers, and ensure that the cement is fully hydrated to form a denser structure, reduce water absorption, and enhance the compression, flexural and antifreeze properties.
[0083] S3 medium-high speed stirring at 290-310r / min for 3-5 minutes can ensure that the fibers are evenly dispersed in the slurry, avoid fiber agglomeration, and form a fiber network. The evenly dispersed fiber network can effectively inhibit the generation and expansion of microcracks, significantly improve the crack resistance, impact resistance and frost resistance of the board, and reduce water absorption.
[0084] In S4, the mixing is also carried out at a high speed of 290-310r / min for 3-5 minutes to ensure that all aggregate components are completely and evenly mixed to form a mixture with a uniform texture. This step helps to optimize the multi-level filling structure of the board, increase its density and compressive strength, reduce water absorption, and further improve its compressive, flexural and frost resistance.
[0085] If the speed in S1 is lower than the recommended 45r / min, the dry powder components will not be fully mixed, agglomeration will occur, and the uniformity of the subsequent slurry and the performance of the board will be affected. The stirring speed is too high: If the speed exceeds 55r / min, the dry powder components will be over-crushed, affecting the particle size distribution, thereby affecting the structural properties and appearance of the final board. The stirring time is too short: A stirring time of less than 1 minute will result in uneven mixing, while a time that is too long (more than 2 minutes) will cause excessive stirring of the powder, resulting in unnecessary energy consumption and equipment wear.
[0086] The stirring speed in S2 is too low: the initial medium-speed stirring (less than 140r / min) and the later high-speed stirring (less than 290r / min) result in insufficient mixing of the liquid and dry powder components, affecting the fluidity of the slurry and the strength of the final board. The stirring speed is too high: the initial speed is too high (more than 160r / min) and introduces too much air, forming a large number of bubbles, affecting the density and strength of the board; the later speed is too high (more than 310r / min) and destroys the slurry structure and reduces its viscosity. The stirring time is too short or too long: too short time (less than 0.4 minutes in the early stage or less than 3 minutes in the later stage) results in insufficient mixing of the components, and too long time (more than 0.6 minutes in the early stage or more than 5 minutes in the later stage) introduces too much shear force, destroys the structure of the slurry and affects the fiber distribution.
[0087] The stirring speed in S3 is too low: a speed lower than 290r / min cannot effectively disperse the fibers, resulting in fiber agglomeration, which affects the crack resistance and impact resistance of the board. The stirring speed is too high: a speed exceeding 310r / min damages the fibers, reduces their reinforcing effect, and introduces too many bubbles, affecting the performance of the board. The stirring time is too short: less than 3 minutes cannot ensure that the fibers are fully dispersed, while a time that is too long (more than 5 minutes) destroys the fiber structure and reduces its reinforcing effect.
[0088] The stirring speed in S4 is too low: a speed lower than 290r / min will result in uneven mixing of aggregates, affecting the structural strength and appearance of the board. The stirring speed is too high: a speed exceeding 310r / min will damage the aggregates, affecting their original size distribution, and thus affecting the performance of the board. The stirring time is too short or too long: a time that is too short (less than 3 minutes) will result in insufficient mixing, while a time that is too long (more than 5 minutes) will introduce unnecessary shear force, affecting the structure and performance of the slurry.
[0089] In summary, exceeding the recommended mixing parameter range will lead to various problems in the preparation process of inorganic artificial stone slabs, including uneven mixing, performance degradation, increased energy consumption, and equipment wear, which will affect the quality of the final product and production efficiency. Therefore, following precise mixing parameters is crucial to ensure the performance of inorganic artificial stone slabs and the smooth progress of the production process.
[0090] Furthermore, the parameters of the press-molded rough board in step S5 are: vacuum degree of -0.093 to -0.097 MPa, pressing pressure of 10-15 MPa, holding time of 100s-120s; the pressing process is accompanied by vibration, the vibration frequency is 30-40Hz, 2-3min.
[0091] Furthermore, in step S6, the pressed rough board is initially cured for 22-26 hours in an environment with a temperature of 18-25° C. and a humidity of not less than 95%, and then demolded;
[0092] After demoulding, the rough board enters the closed spray curing stage, maintaining the ambient temperature at 18-25℃ and the humidity not less than 95%, and the curing lasts for at least 14 days.
[0093] Setting the vacuum degree to -0.093 to -0.097 MPa and the holding time to 100s-120s can effectively remove the air inside the board, reduce the porosity, and increase the density and strength of the board. This helps to reduce water absorption, enhance anti-freezing properties, and improve compression, flexural and ball impact resistance.
[0094] Applying a pressure of 10-15MPa and a vibration frequency of 30Hz for 2-3 minutes helps to ensure the uniform distribution of the internal components of the board, promotes the close bonding of the fibers and the matrix material, and accelerates the discharge of moisture, further improving the density and strength of the board.
[0095] The initial curing for 22-26 hours in an environment with a temperature of 18-25℃ and a humidity of not less than 95% provides ideal conditions for the hydration reaction of cement. Such an environment helps the cement to fully hydrate, form a stronger hardened body, and improve the structural stability and compressive strength of the board.
[0096] Continuous curing for at least 14 days at a temperature of 18-25°C and a humidity of not less than 95% can further promote the hydration process of cement and enhance the mechanical properties of the board. Spraying can keep the surface of the board moist, avoid cracking caused by rapid evaporation of surface moisture, and help improve the durability and crack resistance of the board.
[0097] (III) Beneficial effects
[0098] The beneficial effects of the present invention are as follows: the present invention proposes a non-polar artificial stone board and its preparation process, which aims at solving the problem of uneven dispersion of fibers in the artificial stone matrix in the prior art, and the resulting defects such as inconsistent mechanical properties of the board, weak compression and flexural properties, poor falling ball impact resistance, poor frost resistance and high water absorption, and significantly improves the comprehensive performance of the artificial stone board through innovative formula design.
[0099] Through the improved mixing process and specific fiber length ratio (6mm in length as the main component, 8mm in length as the auxiliary component, and 10mm in length as the trace component), the uniform distribution of fibers in the matrix is ensured, fiber agglomeration is avoided, and the crack resistance, impact resistance and frost resistance of the board are significantly improved.
[0100] The water-to-gel ratio between water and gel material is strictly controlled at 0.15-0.20, achieving dual optimization of mechanical properties and construction performance, improving the strength and density of the hardened body, reducing water absorption, and enhancing the ability to resist freeze-thaw cycles and corrosion resistance.
[0101] The comprehensive use of calcium sand of different mesh sizes (from coarse to fine) forms a continuous skeleton structure with multi-level filling, which improves the compressive strength, flexural strength, crack resistance and impermeability of the board, while optimizing the fluidity and processability of the board.
[0102] Precisely controlling the mass fraction of each raw material component achieves the best balance between performance and cost, which not only improves the overall performance of the board but also ensures the economical production cost.
[0103] Through the uniform distribution of fibers, optimized water-cement ratio and multi-level filling strategy, the board's compression, flexural resistance, falling ball impact resistance and frost resistance are significantly enhanced, while the water absorption rate is significantly reduced, thereby improving the board's waterproof performance and durability. DETAILED DESCRIPTION
[0104] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below in conjunction with specific embodiments. Unless otherwise specified, the "parts" in the following embodiments refer to parts by mass.
[0105] Example 1
[0106] This embodiment provides a preparation process of a non-polar artificial stone plate, which specifically includes the following steps:
[0107] S1. Mix 21 parts of white silicate cement, 2 parts of active agent, 0.2 parts of inorganic pigment and calcium sand aggregate with a particle size of 10 mesh and 20 mesh accounting for 33% of the total calcium sand mass, including 12 parts of 10 mesh calcium sand and 5 parts of 20 mesh calcium sand, and perform preliminary dry mixing at a stirring speed of 45r / min for 1 minute to ensure uniform mixing.
[0108] S2. Add 1 part of water reducing agent, 1.5 parts of water and 5 parts of toughening agent to the mixture in step S1, control the water-binder ratio to 0.18, and stir again, first stirring at a speed of 140 r / min for 0.4 min, then stirring at a speed of 300 r / min for 4 min, to ensure that all liquids and dry powders are fully mixed to form a uniform slurry.
[0109] S3, add pre-weighed fibers of 6 mm, 8 mm and 10 mm in length to step S2, the fiber distribution ratio is 60% of the total fiber mass of 6 mm, 39.6% of the total fiber mass of 8 mm, and 0.4% of the total fiber mass of 10 mm, wherein the total fiber amount is 0.6 parts, continue stirring for 5 minutes, the stirring speed is 300r / min, and ensure that the fibers are evenly dispersed in the slurry. Among them, the fiber is glass fiber.
[0110] S4. Add the remaining calcium sand aggregate to the slurry of step S3, and stir again at a stirring speed of 300 r / min for 4 minutes until all ingredients are completely and evenly mixed to form a mixture with a uniform texture; wherein the remaining calcium sand aggregate has specifications of 40 mesh calcium sand, 5 parts; 60 mesh calcium sand, 3 parts; 80 mesh calcium sand, 10 parts; 100 mesh calcium sand, 12 parts; 325 mesh calcium sand, 5 parts.
[0111] S5. Fill the uniform mixture in step S4 into the mold and press it under vacuum to form a rough board; the vacuum degree is -0.093MPa, the pressure is 12MPa, the holding time is 110s, and the pressing process is accompanied by vibration, the vibration frequency is 30Hz, and the duration is 2min.
[0112] S6, curing the rough board after pressing and forming in step S5; curing the pressed rough board in an environment with a temperature of 25° C. and a humidity of 95% for 24 hours, and then demolding;
[0113] After demoulding, the panels enter the closed spray curing stage, maintaining an ambient temperature of 25°C and a humidity of 95% for 28 days.
[0114] The water-cement ratio is calculated as the total water content / the total amount of gel material. For example, the mass of water added is 1.5 parts, white silicate cement is 21 parts, active agent is 2 parts, organic additive is 5 parts, and water reducer is 1 part. Among them, the water content of organic additive is 50%, the water content of water reducer is 60%, the water content of organic additive is 2.5 parts, the solid content of organic additive is 2.5 parts, the water content of water reducer is 0.6 parts, and the solid content of water reducer is 0.4 parts. Therefore, the total water content is 4.6 parts, the total gel content is 25.9 parts, and the water-cement ratio is approximately equal to 0.18.
[0115] Example 2
[0116] The difference between this embodiment and embodiment 1 is that in step S3, the fiber distribution ratio is 6 mm fiber mass accounts for 70% of the total fiber mass, 8 mm fiber mass accounts for 29.8% of the total fiber mass, and 10 mm fiber mass accounts for 0.2% of the total fiber mass, wherein the total fiber amount is 0.6 parts.
[0117] Example 3
[0118] The difference between this embodiment and embodiment 1 lies in steps S1 and S4, wherein:
[0119] S1. Mix 21 parts of white silicate cement, 2 parts of active agent, 0.2 parts of inorganic pigment and calcium sand aggregate with a particle size of 10 mesh and 20 mesh accounting for 30% of the total calcium sand mass, including 15 parts of 10 mesh calcium sand and 7 parts of 20 mesh calcium sand, and conduct preliminary dry mixing at a stirring speed of 45r / min for 1 minute to ensure uniform mixing.
[0120] S4. Add the remaining calcium sand aggregate to step S3, and stir again at a stirring speed of 300 r / min for 4 minutes, until all ingredients are completely and evenly mixed to form a mixture with a uniform texture; wherein the remaining calcium sand aggregate has specifications of 40 mesh calcium sand, 8 parts; 60 mesh calcium sand, 4 parts; 80 mesh calcium sand, 15 parts; 100 mesh calcium sand, 17 parts; and 325 mesh calcium sand, 7 parts.
[0121] Comparative Example 1
[0122] The proportions of the ingredients were the same as in Example 1, but without the addition of fiber.
[0123] Comparative Example 2
[0124] According to the proportions of the components in Example 1, all glass fibers with a length of 6 mm were added.
[0125] Comparative Example 3
[0126] The difference between this comparative example and Example 1 is that the water-cement ratio is 0.23, wherein, for example, the mass of water is 3 parts, the mass of white silicate cement is 24 parts, the mass of active agent is 2 parts, the mass of organic additive is 5 parts, the mass of water reducer is 2 parts, the mass of water content of organic additive is 50%, the mass of water reducer is 60%, the mass of water content of organic additive is 2.5 parts, the mass of solid content in organic additive is 2.5 parts, the mass of water reducer is 1.2 parts, and the mass of solid content in water reducer is 0.8 parts. Therefore, the total water content is 6.7 parts, the total gel content is 29.3 parts, and the water-cement ratio is approximately equal to 0.23.
[0127] Comparative Example 4
[0128] The difference between this comparative example and Example 1 is that: in S1, the stirring speed is 60 r / min, and the stirring time is 3 min; in S2, the stirring speed is first 170 r / min, and the stirring time is 0.8 min, and then the stirring speed is 320 r / min, and the stirring time is 7 min; in S3 and S4, the stirring speeds are both 320 r / min, and the stirring time is both 6 min.
[0129] The compression resistance, flexural resistance, falling ball impact resistance, frost resistance and water absorption of the inorganic artificial stone slabs cured for 28 days were tested. The test results are shown in the table below.
[0130]
[0131]
[0132] Example 2 keeps the total fiber amount at 0.6 parts, but adjusts the distribution ratio of fiber length, that is, 6mm fiber accounts for 70% of the total fiber mass, 8mm fiber accounts for 29.8%, and 10mm fiber accounts for 0.2%. This change causes a slight decrease in compressive strength to 89.0MPa, flexural strength to 14.7MPa, ball impact resistance to 3.4J, frost resistance to -10.5%, and water absorption to 0.16%. Although the change in fiber length distribution has limited effect on performance, it can be seen that the compressive strength, flexural strength and ball impact resistance have decreased slightly. This is due to the reduction in the proportion of 8mm and 10mm fibers, which reduces the ability of the board to disperse stress when impacted, as well as the fiber "bridge" effect of flexural performance.
[0133] In Example 3, the proportion of 10-mesh and 20-mesh calcium sand was adjusted to 30% of the total calcium sand mass, and the remaining calcium sand aggregate ratio was adjusted, resulting in slight fluctuations in compressive strength and flexural strength, which were 89.2 MPa and 14.8 MPa, respectively, and the ball impact resistance remained at 3.4 J. This shows that the fine-tuning of the calcium sand ratio within the range has a limited effect on the performance of the board, and the overall performance of the board remains stable.
[0134] The compressive strength of Example 1 is significantly higher than that of Comparative Example 1. The addition of fibers can significantly improve the compressive strength of the board. The fibers form a network structure during the cement hardening process, which can effectively disperse stress and avoid stress concentration, thereby improving the ability of the board to resist compressive loads. The "bridge" effect of the fibers allows stress to be more evenly distributed when under pressure, reducing the formation and development of microcracks, thereby improving the compressive strength. The flexural strength of Example 1 is better than that of Comparative Example 1. The fibers act as reinforcing ribs in the board, which can resist tensile stress and effectively prevent the expansion of cracks. When the board is subjected to a bending load, the fibers can cross the cracks to form a "bridge", thereby improving the bending resistance of the board. The addition of fibers increases the toughness of the board, enabling it to better absorb energy when subjected to force and avoid brittle fracture, thereby improving the flexural strength. The falling ball impact resistance of Example 1 is significantly higher than that of Comparative Example 1. The uniform distribution of fibers and the fiber network structure can effectively absorb and disperse impact energy, reduce stress concentration points, and prevent the board from breaking due to excessive local stress. The addition of fibers improves the toughness and elastic modulus of the board, so that the board can be better deformed and restored to its original shape when impacted, reducing the damage to the board structure caused by the impact and improving the resistance to falling ball impact. The frost resistance of Example 1 is better than that of Comparative Example 1. The addition of fibers can improve the microstructure of the board and reduce the porosity, thereby improving the density of the board. In a low temperature environment, the expansion force generated when water freezes inside the board will damage the board structure. Fibers can fill tiny pores and reduce the penetration of water. At the same time, the fiber network structure can absorb the stress caused by the expansion of ice crystals, reduce the risk of damage to the board during the freeze-thaw cycle, and improve the frost resistance. The water absorption rate of Example 1 is lower than that of Comparative Example 1. The addition of fibers can improve the microstructure of the board, form a denser structure, and reduce the penetration channel of water. The composite structure formed by fibers and cement hydration products can block the penetration of water and reduce the water absorption rate of the board. Low water absorption not only improves the waterproof performance of the board, but also indirectly improves the frost resistance and durability, because the water reduces the destructive effect of the freeze-thaw cycle on the board.
[0135] In Example 1, the fiber length distribution is carefully designed, including three different lengths of fibers, 6 mm, 8 mm and 10 mm, and each of them occupies a specific proportion. This multi-level fiber ratio strategy makes full use of the unique role of fibers of different lengths to form a complex and effective fiber network, thereby significantly improving the overall performance of the board. In contrast, Comparative Example 2 only uses fibers with a length of 6 mm, ignoring the synergy between fibers of different lengths, resulting in performance differences. In Example 1, fibers of different lengths work together to form a more complex and more effective stress transfer network. Fibers with a length of 6 mm are used as the main fibers, providing basic strength and crack resistance; fibers with a length of 8 mm and a length of 10 mm are used as auxiliary and trace fibers, respectively, to enhance impact resistance and antifreeze performance, while optimizing crack resistance. In Comparative Example 2, only fibers with a length of 6 mm are used, lacking the "bridge" effect of longer fibers, resulting in a weakened stress dispersion ability and a decrease in compressive strength. The flexural strength of Example 1 is higher than that of Comparative Example 2, and the improvement in flexural strength is also due to the synergy of fibers of different lengths. When subjected to bending load, the fibers with a length of 8 mm and a length of 10 mm can provide additional support, prevent the expansion of cracks, and improve the toughness of the board. In comparative example 2, due to the lack of such a multi-level fiber network, the flexural resistance is affected to a certain extent. The falling ball impact resistance of Example 1 is better than that of comparative example 2. When subjected to impact, the fibers with a length of 8 mm and a length of 10 mm can absorb and disperse more impact energy, reduce stress concentration, and prevent the board from being broken due to excessive local stress. In comparative example 2, only relying on the 6 mm fiber, its ability to absorb impact energy is limited, resulting in a decrease in falling ball impact resistance. The comparison between Example 1 and comparative example 2 clearly shows that the synergistic effect of fibers of different lengths is crucial to improving the comprehensive performance of inorganic artificial stone boards. By rationally designing the fiber length distribution, an efficient, multi-level fiber network can be formed to effectively improve the compressive strength, flexural strength and falling ball impact resistance of the board. Ignoring the diversity of fiber length and using only fibers of a single length will lead to a decrease in board performance, especially the impact on impact resistance and flexural resistance.
[0136] The water-cement ratio is one of the key parameters that determine the performance of concrete or artificial stone panels. The optimized water-cement ratio can significantly improve the mechanical properties and waterproof properties of the panels, while the higher water-cement ratio (0.23) in Comparative Example 3 leads to a decrease in performance. The compressive strength of Example 1 is much higher than that of Comparative Example 3. The low water-cement ratio helps to form a denser hardened structure and reduce porosity, thereby improving the compressive strength. On the contrary, the higher water-cement ratio of Comparative Example 3 leads to more pores and microcracks in the hardened structure, reducing the compressive strength. The flexural strength of Example 1 is also better than that of Comparative Example 3. The dense structure formed by the low water-cement ratio reduces the formation of microcracks and improves the ability of the panel to resist bending loads. The higher water-cement ratio of Comparative Example 3 reduces the density of the hardened body and increases the microcracks inside the panel, thereby reducing the flexural strength. The falling ball impact resistance of Example 1 is higher than that of Comparative Example 3. The low water-cement ratio helps to form a tougher structure and improves the ability of the panel to absorb and disperse impact energy. The higher water-cement ratio of Comparative Example 3 reduces the toughness of the structure and reduces the ability of the panel to absorb impact energy, thereby reducing the falling ball impact resistance. The water absorption rate of Example 1 is significantly lower than that of Comparative Example 3. The low water-cement ratio helps to form a denser structure, reduces the channels for water penetration, and thus reduces the water absorption rate. The higher water-cement ratio of Comparative Example 3 increases the pores in the structure, provides more paths for water penetration, and improves the water absorption rate. The frost resistance of Example 1 is better than that of Comparative Example 3. The dense structure formed by the low water-cement ratio reduces the damage to the board caused by the freezing and expansion of water at low temperatures, and improves the frost resistance. The higher water-cement ratio of Comparative Example 3 increases the moisture content inside the board, which has a greater destructive effect on the structure when freezing and expanding, and reduces the frost resistance. The comparison between Example 1 and Comparative Example 3 clearly shows the importance of the optimized water-cement ratio to improve the mechanical properties and waterproof properties of inorganic artificial stone boards. The low water-cement ratio helps to form a denser and tougher hardened structure, improves the compressive strength, flexural strength and falling ball impact resistance, while reducing the water absorption rate and improving the frost resistance. In contrast, a higher water-cement ratio leads to more pores and microcracks in the hardened structure, reducing the overall performance of the board.
[0137] The change of mixing process parameters has a significant impact on the performance of inorganic artificial stone board. Example 1 uses precise mixing process parameters, while Comparative Example 4 changes these parameters, resulting in differences in board performance. The compressive strength of Example 1 is higher than that of Comparative Example 4. The precisely controlled mixing process ensures the uniform distribution of fibers in the mixture, forming a uniform and dense structure, thereby improving the compressive strength. The changed mixing process parameters in Comparative Example 4 affect the distribution of fibers, resulting in areas with uneven fiber distribution in the structure, which reduces the compressive strength. The flexural strength of Example 1 is higher than that of Comparative Example 4. The uniform distribution of fibers is crucial to improving the flexural strength because it can effectively prevent or delay the expansion of cracks. The change of mixing process parameters in Comparative Example 4 affects the uniform dispersion of fibers, reduces the ability of the board to resist bending loads, and thus reduces the flexural strength. The falling ball impact resistance of Example 1 is higher than that of Comparative Example 4. The uniform distribution of fibers improves the toughness of the board and can more effectively absorb and disperse impact energy. The change of mixing process parameters in Comparative Example 4 affects the formation of the fiber network, reduces the ability of the board to absorb impact energy, and thus reduces the falling ball impact resistance. The water absorption rate of Example 1 is lower than that of Comparative Example 4. The uniform distribution of fibers helps to form a dense structure, reduces the channels for water penetration, and reduces the water absorption rate. The change of the stirring process parameters in Comparative Example 4 affects the density of the structure, increases the chance of water penetration, and thus improves the water absorption rate. Therefore, the optimized stirring process helps the fibers to be evenly dispersed in the mixture, forming a uniform and dense structure, improving the compressive strength, flexural strength and ball impact resistance, while reducing the water absorption rate. In contrast, the change of the stirring process parameters leads to uneven fiber distribution and reduces the comprehensive performance of the board. Therefore, precise control of the stirring process parameters is one of the key factors to improve the performance of inorganic artificial stone boards.
[0138] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. An inorganic artificial stone plate, which is made by beating powder and calcium sand with particle sizes of 10 mesh and 20 mesh into slurry under the action of an auxiliary agent, and then adding aggregates to form a vacuum vibration pressing, wherein the slurry includes silicate cement, inorganic pigments and calcium sand with particle sizes of 10 mesh and 20 mesh, the auxiliary agent includes an active agent, a water reducer and a toughening agent, and the aggregate includes calcium sand with particle sizes of 40 mesh, 60 mesh, 80 mesh, 100 mesh and 325 mesh and fiber; The artificial stone plate comprises the following components: The calcium sand with a particle size of 10 mesh has a mass fraction of 10-20 parts; The calcium sand with a particle size of 20 mesh has a mass fraction of 5-10 parts; The calcium sand with a particle size of 40 mesh has a mass fraction of 5-8 parts; The calcium sand with a particle size of 60 mesh has a mass fraction of 3-4 parts; The calcium sand with a particle size of 80 mesh has a mass fraction of 10-15 parts; The calcium sand with a particle size of 100 mesh has a mass fraction of 12-17 parts; The calcium sand with a particle size of 325 mesh has a mass fraction of 5-7 parts; Active agent, the mass fraction thereof is 2-5 parts; Inorganic pigment, its mass fraction is 0.1-0.5 parts; Fiber, the mass fraction thereof is 0.2-0.6 parts; Portland cement, 20-30 parts by mass; Water reducing agent, the mass fraction thereof is 1-2 parts; Toughening agent, its weight proportion is 2-5 parts.
2. The inorganic artificial stone plate according to claim 1, characterized in that: The fiber length is 6-10 mm, of which the fiber with a length of 6 mm accounts for 60%-70% of the total fiber mass, the fiber with a length of 8 mm accounts for 29.8%-39.6% of the total fiber mass, and the fiber with a length of 10 mm accounts for 0.2%-0.4% of the total fiber mass; The fiber is polypropylene fiber or glass fiber.
3. The inorganic artificial stone plate according to claim 1, characterized in that: Calcium sand with particle sizes of 10 mesh and 20 mesh accounts for 27%-34% of the total calcium sand mass.
4. The inorganic artificial stone plate according to claim 1, characterized in that: The toughening agent is at least one of styrene-butadiene emulsion, silicone-acrylic emulsion and pure acrylic emulsion.
5. The inorganic artificial stone plate according to claim 1, characterized in that: The active agent is at least one of white fly ash, white silica fume and metakaolin.
6. The inorganic artificial stone plate according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid water reducing agent.
7. The process for preparing the inorganic artificial stone plate according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Mix silicate cement, active agent, inorganic pigment and calcium sand with specifications of 10 mesh and 20 mesh accounting for 27%-34% of the total calcium sand mass, perform preliminary dry mixing, and stir evenly; S2. Add water reducing agent, water and toughening agent to the mixture of step S1, control the water-binder ratio to 0.15-0.20, and stir at different speeds to ensure that all liquids and dry powders are fully mixed to form a uniform slurry; S3, adding fibers with a specification of 6 mm-10 mm to the slurry in step S2, wherein the fibers with a length of 6 mm account for 60%-70% of the total fiber mass, the fibers with a length of 8 mm account for 29.8%-39.6% of the total fiber mass, and the fibers with a length of 10 mm account for 0.2%-0.4% of the total fiber mass, and continue stirring to ensure that the fibers are evenly dispersed in the slurry; S4, adding the remaining calcium sand aggregate to the slurry in step S3, and stirring again until all the ingredients are completely and evenly mixed to form a mixture with a uniform texture; S5, filling the mixed material in step S4 into a mold, and pressing and forming a rough board under vacuum; S6. Curing the rough board after being pressed and formed in step S5.
8. The preparation process according to claim 7, characterized in that: In S1, the stirring speed is 45-55r / min, and the stirring time is 1-2min; in S2, the stirring speed is first 140-160r / min, the stirring time is 0.4-0.6min, and then the stirring speed is 290-310r / min, and the stirring time is 3-5min; in S3 and S4, the stirring speeds are both 290-310r / min, and the stirring time is both 3-5min.
9. The preparation process according to claim 7, characterized in that: The parameters for pressing the rough board in step S5 are: vacuum degree of -0.093 to -0.097 MPa, pressing pressure of 10-15 MPa, holding time of 100s-120s; vibration is accompanied during the pressing process, the vibration frequency is 30-40Hz, 2-3min.
10. The preparation process according to claim 7, characterized in that: In step S6, the pressed rough board is initially cured for 22-26 hours in an environment with a temperature of 18-25° C. and a humidity of not less than 95%, and then demolded; After demoulding, the rough board enters the closed spray curing stage, maintaining the ambient temperature at 18-25℃ and the humidity not less than 95%, and the curing lasts for at least 14 days.
Citation Information
Cited By
Rapid curing process of geopolymer-based material
CN120364963A