Near-full-solid-waste semi-rigid base layer and laying method thereof
By introducing pellet-based flexible base layers and rigid grouting layers into the semi-rigid base layer, combining specific material ratios to form a semi-flexible and semi-rigid structure, the problems of prone to cracks and fatigue of flexible base layers are solved, and high-grade highways are realized High load-bearing capacity and water loss resistance.
Patent Information
- Application Number
- CN202411116928.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
AI Technical Summary
The existing semi-rigid base layer is prone to cracks under the effects of temperature shrinkage, dry shrinkage, etc., which leads to damage to the pavement structure. The increase in the thickness of the asphalt surface cannot effectively reflect the advantages of compressive strength, and the flexible base layer is prone to fatigue and cracking under bending tensile stress. It is difficult to meet the bearing capacity and water damage resistance requirements of high-grade highways.
Adopt nearly all solid waste semi-rigid base structure, including pellet-based flexible base layer and rigid grouting layer poured into it, and form semi-flexible through specific proportions of steel slag, desulfurization ash, ore powder, rubber powder and white mud. Semi-rigid base layer, increasing the strength of the base layer and improving the flexibility of the grouting material, avoiding cracking and water damage.
It achieves high load-bearing capacity, excellent water loss resistance and mechanical properties without reflective cracks. It is suitable for highways and heavy traffic loads, avoiding fatigue and cracking problems in traditional semi-rigid bases, and reducing investment costs.
Smart Images

Figure BDA0004993891290000031 
Figure BDA0004993891290000041 
Figure BDA0004993891290000051
Abstract
Description
Technical Field
[0001] The invention belongs to the field of road base preparation, and in particular relates to a nearly all-solid waste semi-rigid base and a paving method thereof. Background Art
[0002] More than 90% of the structures of my country's high-grade highways are semi-rigid base asphalt pavements. The use of semi-rigid base can effectively increase the bearing capacity of the pavement and provide stable support for the surface layer. However, due to the insurmountable shortcomings of the semi-rigid base itself, temperature shrinkage, dry shrinkage, cracks, and eventually reflective cracks, under the combined effects of driving loads, water, and temperature gradients, the pavement structure will produce slurry, looseness and other diseases, eventually leading to the destruction of the pavement structure. In order to prevent reflective cracks, the common practice is to increase the thickness of the asphalt surface layer, but as the thickness of the asphalt surface layer increases, the cost increases accordingly, and the advantages of the high compressive strength of the semi-rigid base cannot be effectively reflected.
[0003] Flexible materials such as graded crushed stone and asphalt stabilized crushed stone are viscoelastic materials with good toughness and certain self-healing ability, but they have large deformation and deflection, so the pavement thickness is also large and the investment cost is also high. In the flexible base pavement structure, the tensile stress at the bottom of the base layer is the largest, and the possibility of fatigue cracking at the bottom of the layer under the repeated action of bending and tensile stress is also the greatest. Therefore, the base layer is required to have good durability, especially excellent fatigue resistance, and as a load-bearing layer, it is required to have a certain anti-rutting ability. Due to the low bearing capacity, flexible base layers such as graded crushed stone are generally used to pave the subbase or the leveling layer on the roadbed to strengthen the roadbed.
[0004] Therefore, there is an urgent need for a new type of base structure suitable for high-grade highway asphalt pavement to achieve high bearing capacity, good water damage resistance and no reflective cracks. Summary of the invention
[0005] Purpose of the invention: The technical problem to be solved by the present invention is to provide a new type of base structure to achieve mechanical properties of high bearing capacity, good water damage resistance and no reflective cracks.
[0006] Technical solution: The nearly solid waste semi-rigid base of the present invention comprises a granular flexible base and a rigid grouting layer poured into the granular flexible base;
[0007] The raw materials used for the rigid grouting layer include 42-50% of component A, 30-38% of component B and 20-25% of water by mass fraction; wherein, component A includes 20-30% of steel slag, 8-12% of desulfurized ash, 35-45% of mineral powder, 12-20% of sulphoaluminate cement clinker and 3-4% of admixture by mass fraction; component B includes 15-25% of rubber powder and 75-85% of white mud by mass fraction.
[0008] The present invention is based on nearly all-solid waste granular flexible materials and grouting materials, and adopts the form of flexible base layer poured with rigid materials to form a semi-flexible and semi-rigid base layer. It not only increases the strength of the granular flexible base layer, but also can be suitable for the pavement base layer of highways and heavy traffic load requirements. At the same time, it avoids the defects of traditional semi-rigid base materials that are prone to fatigue and shrinkage and freezing cracking, which lead to reflective cracks and water damage in the pavement.
[0009] Among them, the grouting layer belongs to a semi-flexible and semi-rigid base layer. The addition of materials such as rubber powder improves the flexibility of the grouting material, so that the surface of the base layer is firmly bonded to the asphalt concrete surface layer; and the grouting material adopts component B compounded by rubber powder and white mud. When it is compounded with component A composed of steel slag, desulfurization ash, mineral powder, sulfoaluminate cement clinker and admixtures and water to form a slurry, on the one hand, the alkalinity of the white mud changes the rubber powder from hydrophobic to hydrophilic, and after mixing with component A and water, the bonding between the rubber powder and the slurry interface is improved; on the other hand, due to alkaline erosion, cracks are generated on the surface of the rubber powder. During the mixing process of the slurry, the slurry will penetrate into the cracks of the rubber powder to improve the strength of the grouting material.
[0010] Furthermore, the raw materials used in the granular flexible base of the nearly all-solid waste semi-rigid base are graded crushed stone, graded gravel, natural gravel or concrete pavement crushed stone with a void ratio of 20-25% after compaction and a maximum particle size of ≤37.5mm.
[0011] Furthermore, the admixtures used in the nearly all-solid waste semi-rigid base layer include 20-35% of polycarboxylic acid water-reducing agent, 55-65% of sodium sulfate and 10-25% of calcium formate by mass fraction.
[0012] Furthermore, the specific surface area of the steel slag, desulfurization ash, mineral powder, sulphoaluminate cement clinker and carbide slag used in the nearly all-solid waste semi-rigid base is ≥400kg / m 2 .
[0013] Furthermore, the particle size of the rubber powder used in the nearly all-solid waste semi-rigid base layer is 70-120 meshes.
[0014] The preparation method of the nearly all-solid waste semi-rigid base grouting material of the present invention comprises the following steps:
[0015] (1) Steel slag, desulfurized ash, mineral powder, sulphoaluminate cement clinker and admixtures are mixed and stirred to obtain component A;
[0016] (2) Mixing and stirring rubber powder and white mud to obtain component B;
[0017] (3) Component A, component B and water are mixed and stirred uniformly to obtain the grouting material.
[0018] The method for laying the above-mentioned nearly all-solid waste semi-rigid base layer of the present invention comprises the following steps:
[0019] (1) Spread granular flexible base and control the loose paving coefficient to 1.15-1.35;
[0020] (2) rolling the above-mentioned granular flexible base to ensure that the void ratio after rolling reaches 20-25%;
[0021] (3) Pour the grouting material into the gaps of the granular flexible base layer, scrape off the surface slurry, and maintain the base layer.
[0022] Beneficial effects: Compared with the prior art, the significant advantages of the present invention are: the nearly all-solid waste semi-rigid base layer adopts the form of a flexible base layer poured with rigid materials, which increases the strength of the granular flexible base layer and can be used for the pavement base layer required by highways and heavy traffic loads, while avoiding the defects of traditional semi-rigid base materials that are prone to fatigue and shrinkage and freezing cracking, resulting in reflective cracks and water damage in the pavement. DETAILED DESCRIPTION
[0023] The technical solution of the present invention is further described in detail below in conjunction with embodiments.
[0024] The nearly solid waste semi-rigid base layer of the present invention comprises a granular flexible base layer with a void ratio of 20-25% after compaction and a maximum particle size of ≤37.5mm and a rigid grouting layer poured into the granular flexible base layer.
[0025] Among them, the raw materials used for the granular flexible base layer can be graded crushed stone, graded gravel, natural gravel or crushed concrete pavement.
[0026] The raw materials used for the rigid grouting layer include 42-50% of component A, 30-38% of component B and 20-25% of water by mass fraction. Component A includes 20-30% of steel slag, 8-12% of desulfurization ash, 35-45% of mineral powder, 12-20% of sulphoaluminate cement clinker and 3-4% of admixture by mass fraction; component B includes 15-25% of rubber powder and 75-85% of white mud by mass fraction. Among them, the chemical composition of steel slag, sulphoaluminate cement clinker and white mud is shown in Table 1 and Table 2. The grade of sulphoaluminate cement is not limited, and it only needs to meet the national standard GB / T37125-2018. The particle size of rubber powder is 70-120 mesh. The specific surface area of steel slag, desulfurization ash, mineral powder, sulphoaluminate cement clinker and carbide slag is ≥400kg / m 2 .
[0027] Table 1 Chemical composition of steel slag and white mud
[0028]
[0029] Example 1
[0030] This embodiment 1 includes a graded crushed stone base with a porosity of 20-25% and a maximum particle size of ≤37.5 mm after compaction, and a rigid grouting layer poured into the graded crushed stone. The components and contents of the raw materials used in the rigid grouting layer are shown in Table 3 below.
[0031] Table 3 Component formula of grouting layer material of Example 1
[0032]
[0033] The content of the admixture components is shown in Table 4 below.
[0034] Table 4 Component contents of the additives of Example 1
[0035] Serial number Components content / % 1 Polycarboxylate water reducer 30 2 Sodium sulfate 60 3 Calcium formate 10
[0036] The method for laying a nearly solid waste semi-rigid base layer of Example 1 comprises the following steps:
[0037] (1) preparing grouting material: mixing and stirring steel slag, desulfurized ash, mineral powder, sulphoaluminate cement clinker and admixtures to obtain component A; mixing and stirring rubber powder and white mud to obtain component B; mixing and stirring component A, component B and water to obtain the grouting material;
[0038] (2) Spread granular flexible base and control the loose paving coefficient to 1.15-1.35;
[0039] (3) rolling the above-mentioned granular flexible base to ensure that the void ratio after rolling reaches 20-25%;
[0040] (4) Pour the grouting material into the gaps of the granular flexible base layer, scrape off the surface slurry, and maintain the base layer.
[0041] Example 2
[0042] This embodiment 2 includes a graded crushed stone base with a porosity of 20-25% and a maximum particle size of ≤37.5 mm after compaction, and a rigid grouting layer poured into the graded crushed stone. The components and contents of the raw materials used in the rigid grouting layer are shown in Table 4 below.
[0043] Table 4 Component formula of grouting layer material of Example 2
[0044]
[0045] Among them, the component contents of the admixtures are shown in Table 5 below.
[0046] Table 5 Component contents of the additives of Example 2
[0047] Serial number Components content / % 1 Polycarboxylate water reducer 20 2 Sodium sulfate 65 3 Calcium formate 15
[0048] The method for laying a nearly solid waste semi-rigid base layer of Example 2 comprises the following steps:
[0049] (1) preparing grouting material: mixing and stirring steel slag, desulfurized ash, mineral powder, sulphoaluminate cement clinker and admixtures to obtain component A; mixing and stirring rubber powder and white mud to obtain component B; mixing and stirring component A, component B and water to obtain the grouting material;
[0050] (2) Spread granular flexible base and control the loose paving coefficient to 1.15-1.35;
[0051] (3) rolling the above-mentioned granular flexible base to ensure that the void ratio after rolling reaches 20-25%;
[0052] (4) Pour the grouting material into the gaps of the granular flexible base layer, scrape off the surface slurry, and maintain the base layer.
[0053] Example 3
[0054] This embodiment 3 includes a graded crushed stone base with a porosity of 20-25% and a maximum particle size of ≤37.5 mm after compaction, and a rigid grouting layer poured into the graded crushed stone. The components and contents of the raw materials used in the rigid grouting layer are shown in Table 6 below.
[0055] Table 6 Component formula of grouting layer material of Example 3
[0056]
[0057] Among them, the component contents of the admixtures are shown in Table 7 below.
[0058] Table 7 Component content of the additives of Example 3
[0059] Serial number Components content / % 1 Polycarboxylate water reducer 35 2 Sodium sulfate 55 3 Calcium formate 10
[0060] The method for laying a nearly all-solid waste semi-rigid base layer of Example 3 comprises the following steps:
[0061] (1) preparing grouting material: mixing and stirring steel slag, desulfurized ash, mineral powder, sulphoaluminate cement clinker and admixtures to obtain component A; mixing and stirring rubber powder and white mud to obtain component B; mixing and stirring component A, component B and water to obtain the grouting material;
[0062] (2) Spread granular flexible base and control the loose paving coefficient to 1.15-1.35;
[0063] (3) rolling the above-mentioned granular flexible base to ensure that the void ratio after rolling reaches 20-25%;
[0064] (4) Pour the grouting material into the gaps of the granular flexible base layer, scrape off the surface slurry, and maintain the base layer.
[0065] Example 4
[0066] This embodiment 4 includes a graded crushed stone base with a porosity of 20-25% and a maximum particle size of ≤37.5 mm after compaction, and a rigid grouting layer poured into the graded crushed stone. The components and contents of the raw materials used in the rigid grouting layer are shown in Table 8 below.
[0067] Table 8 Component formula of grouting layer material of Example 4
[0068]
[0069] Among them, the component contents of the admixtures are shown in Table 9 below.
[0070] Table 9 Component contents of the additives of Example 4
[0071] Serial number Components content / % 1 Polycarboxylate water reducer 20 2 Sodium sulfate 55 3 Calcium formate 25
[0072] The laying method of the nearly solid waste semi-rigid base layer in Example 4 is the same as that in Example 3.
[0073] Example 5
[0074] This embodiment 5 includes a graded crushed stone base with a porosity of 20-25% and a maximum particle size of ≤37.5 mm after compaction, and a rigid grouting layer poured into the graded crushed stone. The components and contents of the raw materials used in the rigid grouting layer are shown in Table 10 below.
[0075] Table 10 Component formula of grouting layer material of Example 5
[0076]
[0077]
[0078] Wherein, the component content of the admixture is the same as that in Example 4.
[0079] The laying method of the nearly solid waste semi-rigid base layer of Example 5 is the same as that of Example 3.
[0080] Comparative Example 1
[0081] The steps are the same as those in Example 5, except that component B uses only 100% white mud. The specific component contents are shown in Table 11 below.
[0082] Table 11 Component formula of grouting layer material of comparative example 1
[0083]
[0084] Performance Testing
[0085] Table 12 Performance test of samples of Examples 1-5 and Comparative Examples
[0086]
[0087] It can be seen from Table 12 that the base structure prepared by the present invention has a rebound modulus of more than 517MPa and a plastic deformation of less than 1.5mm, which can effectively avoid the fatigue and shrinkage cracking of traditional semi-rigid base materials, which may cause reflective cracks in the road surface; the dynamic splitting residual strength ratio can reach more than 93, and has excellent water damage resistance. The dynamic deformation modulus can reach more than 102MPa, the shear strength can reach more than 0.33MPa, and the 7d unconfined compressive strength can reach more than 9.9MPa, that is, it has excellent bearing capacity.
Claims
1. A nearly all-solid waste semi-rigid base layer, characterized in that: The semi-rigid base layer comprises a granular flexible base layer and a rigid grouting layer poured into the granular flexible base layer; The raw materials used for the rigid grouting layer include 42-50% of component A, 30-38% of component B and 20-25% of water by mass fraction; wherein, component A includes 20-30% of steel slag, 8-12% of desulfurized ash, 35-45% of mineral powder, 12-20% of sulphoaluminate cement clinker and 3-4% of admixture by mass fraction; component B includes 15-25% of rubber powder and 75-85% of white mud by mass fraction.
2. The nearly solid waste semi-rigid base layer according to claim 1, characterized in that: The raw materials used in the granular flexible base layer are graded crushed stone, graded gravel, natural sand and gravel or concrete pavement crushed stone with a void ratio of 20-25% after compaction and a maximum particle size of ≤37.5mm.
3. The nearly solid waste semi-rigid base layer according to claim 1, characterized in that: The admixture comprises 20-35% of polycarboxylate water-reducing agent, 55-65% of sodium sulfate and 10-25% of calcium formate by mass fraction.
4. The nearly all-solid waste semi-rigid base layer according to claim 1, characterized in that: The specific surface areas of the steel slag, desulfurized ash, mineral powder, sulphoaluminate cement clinker and carbide slag are all ≥400kg / m 2 .
5. The nearly all-solid waste semi-rigid base layer according to claim 1, characterized in that: The particle size of the rubber powder is 70-120 meshes.
6. The nearly solid waste semi-rigid base layer according to claim 1, characterized in that: The preparation method of the grouting material comprises the following steps: (1) Steel slag, desulfurized ash, mineral powder, sulphoaluminate cement clinker and admixtures are mixed and stirred to obtain component A; (2) Mixing and stirring rubber powder and white mud to obtain component B; (3) Component A, component B and water are mixed and stirred uniformly to obtain the grouting material.
7. A method for laying the nearly solid waste semi-rigid base layer according to claim 1, characterized in that: The steps include: (1) Spread granular flexible base and control the loose paving coefficient to 1.15-1.35; (2) rolling the above-mentioned granular flexible base to ensure that the void ratio after rolling reaches 20-25%; (3) Pour the grouting material into the gaps of the granular flexible base layer, scrape off the surface slurry, and maintain the base layer.
Citation Information
Cited By
Papermaking white mud mixture for pavement base and construction method of papermaking white mud mixture
CN119285313A
Papermaking white mud mixture for road surface base and construction method thereof
CN119285313B