Tungsten tailing sand-steel slag powder solid waste synergistic paste filling material and preparation method thereof
Through the synergistic paste filling technology of tungsten tailings sand, steel slag powder and slag powder, the problem of low utilization of tailings and steel slag resources is solved, cost reduction and resource recycling are achieved, and the comprehensive utilization rate of tungsten tailings is improved. It has significant economic and environmental advantages.
Patent Information
- Application Number
- CN202411199082.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing tailings disposal technology, cement is commonly used as cementitious agent for tailings slurry filling, which is relatively high in cost and the comprehensive utilization rate of steel slag is low, resulting in low comprehensive utilization rate of tungsten tailings and steel slag, resulting in waste of resources and economical pressure.
Use tungsten tailings sand-steel slag powder solid waste synergistic paste filling material, by mixing tungsten tailings sand, steel slag powder and slag powder in a specific proportion, and adding appropriate amount of water to form paste filling material, and use the cementitiousness of steel slag powder to improve filling stability and economicality of materials.
The cost of tailings paste filling is reduced, the comprehensive utilization rate of tungsten tailings, steel slag and slag is improved, and the circular and sustainable development is achieved, with significant economic and environmental advantages.
Smart Images

Figure CN118930206A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of solid waste resource treatment and comprehensive utilization, and in particular to a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material and a preparation method thereof. Background Art
[0002] Tungsten is widely used and is an important strategic metal. However, since tailings often account for 40-99% of the amount of mined ore, there is a huge amount of tailings accumulation in my country. Starting from 2020, the number of tailings ponds in the country will only decrease in principle, and tailings disposal has become a bottleneck restricting the development of the tungsten industry and a key issue for the survival and development of enterprises. Tailings paste filling technology is widely used in tailings disposal and goaf management due to its significant advantages of safety, environmental protection, economy and efficiency. At present, cement is mostly used as a binder for filling materials, which is relatively expensive. In addition, my country's steel production has remained high all year round, and the annual production of steel slag exceeds 150 million tons. On June 1, 2024, the new version of the national mandatory standard GB175-2023 "General Portland Cement" will be implemented, and steel slag will be completely withdrawn from the cement admixture route, which accounts for 50-80% of its total utilization. The comprehensive utilization of steel slag faces a severe situation. Steel slag contains active minerals such as tricalcium silicate, dicalcium silicate, iron, aluminum and acid salts similar to cement, and has hydraulic cementitious properties. In view of this, the present invention gives full play to the cementing property of steel slag powder and provides a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material, which can improve the comprehensive utilization rate of tungsten tailings and steel slag on the one hand, and on the other hand, the cost of steel slag, slag, etc. is relatively low, which can reduce the cost of tailings paste filling material and achieve the effect of reducing costs and increasing efficiency. Summary of the invention
[0003] In view of the shortcomings of the prior art mentioned above, the purpose of the present invention is to provide a tungsten tailings sand-steel slag powder solid waste collaborative paste filling material and a preparation method thereof, so as to improve the comprehensive utilization rate of tungsten tailings and steel slag, reduce the cost of tailings paste filling material, and achieve the effect of reducing costs and increasing efficiency.
[0004] To achieve the above objectives and other related objectives, the present invention is achieved through the following technical solutions.
[0005] The first aspect of the present invention provides a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material, which comprises the following raw materials in parts by weight: 714-854 parts of tungsten tailings sand, 10-43 parts of steel slag powder, 76-154 parts of slag powder, and 300-551 parts of water.
[0006] In some embodiments of the present invention, the water seepage rate of the tungsten tailings sand-steel slag powder solid waste cooperative paste filling material is 1.5%-5%.
[0007] In some embodiments of the present invention, the slump of the tungsten tailings sand-steel slag powder solid waste and paste filling material is 200-260mm.
[0008] In some embodiments of the present invention, the setting time of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material is >10h.
[0009] In some embodiments of the present invention, the uniaxial compressive strength of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material is 0.5-5Mpa.
[0010] In some embodiments of the present invention, the linear shrinkage rate of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material is less than 5%.
[0011] In some embodiments of the present invention, the slurry concentration of the tungsten tailings sand-steel slag powder solid waste and paste filling material is 65%-73%.
[0012] In some embodiments of the present invention, the mass ratio of the tungsten tailings to the sum of the steel slag powder and the slag powder is 1:(5-7).
[0013] In some embodiments of the present invention, the mass ratio of the steel slag powder to the slag powder is 1:(3-9).
[0014] In some embodiments of the present invention, the particle size of the tungsten tailings is 0.05-4 mm.
[0015] In some embodiments of the present invention, the moisture content of the tungsten tailings is less than 12%.
[0016] In some embodiments of the present invention, the ignition loss of the tungsten tailings is less than 10%.
[0017] In some embodiments of the present invention, the free calcium oxide content of the steel slag powder is less than 3%.
[0018] In some embodiments of the present invention, the particle size range of the steel slag powder is <45 μm.
[0019] In some embodiments of the present invention, the screening content of the tungsten tailings with a particle size of less than 0.05 mm is ≤5%; the screening content of the tungsten tailings with a particle size of more than 4 mm is ≤5%.
[0020] In some embodiments of the present invention, the sieved content of the steel slag powder with a particle size of >45 μm is ≤2%.
[0021] The second aspect of the present invention provides a method for preparing a tungsten tailings sand-steel slag powder solid waste collaborative paste filling material, comprising the following steps:
[0022] S1. Weigh tungsten tailings sand, steel slag powder and slag powder according to weight proportion, mix them evenly to obtain dry material;
[0023] S2. Add water to the dry material obtained in step S1, mix well, and obtain tungsten tailings sand-steel slag powder solid waste synergistic paste filling material.
[0024] In some embodiments of the present invention, the mixing in step S1 is performed by stirring with a stirrer for 2-3 minutes.
[0025] In some embodiments of the present invention, the mass ratio of the dry material to water in step S2 is (1.8-2.7):1.
[0026] In some embodiments of the present invention, the mixing in step S2 is performed by stirring with a stirrer, and the stirring time is 3-5 minutes.
[0027] The third aspect of the present invention provides the use of tungsten tailings sand-steel slag powder solid waste synergistic paste filling material as a filling material.
[0028] As described above, the tungsten tailings sand-steel slag powder solid waste synergistic paste filling material and its preparation method of the present invention have the following characteristics:
[0029] Beneficial effects:
[0030] (1) Tungsten tailings sand-steel slag powder solid waste synergistic paste filling material uses tungsten tailings sand, which is rich in source. Large-scale use of tungsten tailings is conducive to reducing the accumulation of tungsten tailings;
[0031] (2) The binder of tungsten tailings sand-steel slag powder solid waste synergistic paste filling material uses steel slag powder and slag powder, and the steel slag and slag solid waste are synergistically recycled. The cost is more economical than cement, which is conducive to circular sustainable development and has a broader application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 Shown is the preparation flow chart of the tungsten tailings sand-steel slag powder solid waste coordinated paste filling material of the present invention. DETAILED DESCRIPTION
[0033] The tungsten tailings sand-steel slag powder solid waste synergistic paste filling material and the preparation method thereof of the present invention are described in detail below.
[0034] The tungsten tailings sand-steel slag powder solid waste synergistic paste filling material of the present invention fully exerts the cementitious property of steel slag powder under the premise of meeting national standards, makes large-scale use of tailings sand from tungsten mining, reduces the accumulation of tungsten tailings, improves the comprehensive utilization rate of steel slag, slag and tungsten tailings, is conducive to circular sustainable development, and has significant economic efficiency. On this basis, the present invention is completed.
[0035] The first aspect of the present invention provides a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material, the tungsten tailings sand-steel slag powder solid waste synergistic paste filling material comprises the following raw materials in parts by weight: 714-854 parts of tungsten tailings sand, 10-43 parts of steel slag powder, 76-154 parts of slag powder, and 300-551 parts of water. The tungsten tailings sand comes from Hunan Xintianling Tungsten Industry Co., Ltd. The steel slag powder comes from Baoshan Iron and Steel. The slag powder comes from Shanghai Baotian New Building Materials Co., Ltd., which meets the S95 grade of GB / T 18046 "Granulated blast furnace slag powder for cement, mortar and concrete". The S95 grade is a highly active slag powder with a seven-day activity index of not less than 70%, suitable for use in cement, mortar and concrete. The water is industrial water or tap water.
[0036] In some embodiments of the present invention, the water seepage rate of the tungsten tailings sand-steel slag powder solid waste synergistic paste filling material is 1.5%-5%, which can be 1.5%-3.1%, 3.1%-3.5%, 3.5%-3.7%, 3.7%-4%, 4%-5%, 3.1%-5%, 3.5%-5% or 3.7%-5%, etc. The water seepage rate is the proportion of water seeped out of the filling slurry when it flows in the filling body to the total volume. Controlling the water seepage rate within the range of 1.5%-5% helps to maintain the stability of the filling body and the engineering effect.
[0037] In some embodiments of the present invention, the slump of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material is 200-260mm, which can be selected as 200-230mm, 230-233mm, 233-235mm, 235-240mm, 240-260mm, 230-235mm, 230-260mm or 235-260mm, etc. The slump of the filling body refers to the flow property generated by its own weight or external force in the stacked state. It reflects the fluidity, pumpability and working performance of the filling body. Under this slump range, the stability, operability and good density of the filling body during the construction process can be ensured, thereby improving the quality of the project and reducing safety risks.
[0038] In some embodiments of the present invention, the setting time of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material is >10h, which can be selected as 10-10.5h, 10.5-11h, 11.5-12h, 12.5-13h, 13-13.5h, 13.5-14h or 14.5-15h, etc.
[0039] In some embodiments of the present invention, the uniaxial compressive strength of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material is 0.5-5Mpa, which can be 0.5-0.7Mpa, 0.7-2.8Mpa, 2.8-3.6Mpa, 3.6-4Mpa, 4-5Mpa or 0.5-3.6Mpa, etc. The uniaxial compressive strength of the filling body is an important indicator to measure its compressive performance, and the uniaxial compressive strength test is usually used to measure the strength of the filling body.
[0040] In some embodiments of the present invention, the linear shrinkage of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material is less than 5%, and can be selected as 1%-1.9%, 1.9%-2.8%, 2.8%-3.7%, 3.7%-4.8%, 4.8%-8%, 1.9%-4.8% or 2.8%-4.8%, etc. The linear shrinkage of the filling material refers to the shrinkage deformation of the filling material slurry during the pipeline transportation process during the filling process, which is usually expressed as a percentage, reflecting the degree of deformation of the filling material slurry during the flow process.
[0041] In some embodiments of the present invention, the slurry concentration of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material is 65%-73%, and can be optionally 65%-68%, 68%-70% or 70%-73%, etc. The slurry concentration within this range not only helps to maintain the fluidity of the filling slurry, ensure the strength and conveying capacity of the filling body, but also ensure the compaction and stability of the filling body.
[0042] In some embodiments of the present invention, the mass ratio of the tungsten tailings to the sum of the steel slag powder and the slag powder is 1:(5-7), which can be optionally 1:(5-5.5), 1:(5.5-6), 1:(6-6.5) or 1:(6.5-7), etc.
[0043] In some embodiments of the present invention, the mass ratio of the steel slag powder to the slag powder is 1:(3-9), which can be optionally 1:(3-4), 1:(4-5), 1:(5-6), 1:(6-7), 1:(7-8) or 1:(8-9), etc.
[0044] In some embodiments of the present invention, the particle size of the tungsten tailings is 0.05-4 mm, which can be 0.05-1 mm, 1-1.5 mm, 1.5-2 mm, 2-2.5 mm, 2.5-3 mm, 3-3.5 mm or 3.5-4 mm, etc. The screening content of tungsten tailings is required to be no more than 5% of <0.05 mm and no more than 5% of >4 mm.
[0045] In some embodiments of the present invention, the moisture content of the tungsten tailings is less than 12%, and can be selected from 1%-2%, 2%-4%, 4%-6%, 6%-8%, 8%-10% or 10%-12%, etc.
[0046] In some embodiments of the present invention, the ignition loss of the tungsten tailings is less than 10%, and can be selected from 1%-2%, 2%-4%, 4%-6%, 6%-8% or 8%-10%, etc.
[0047] In some embodiments of the present invention, the free calcium oxide content of the steel slag powder is less than 3%, and can be optionally 1%-2% or 2%-3%.
[0048] In some embodiments of the present invention, the particle size range of the steel slag powder is <45 μm, which can be 1-10 μm, 10-15 μm, 15-25 μm, 25-30 μm, 30-35 μm, 35-40 μm or 40-45 μm, etc. The screening content of the steel slag powder is required to be greater than >45 μm and not exceed 2%.
[0049] The second aspect of the present invention provides a method for preparing the tungsten tailings sand-steel slag powder solid waste synergistic paste filling material according to the first aspect of the present invention, comprising the following steps:
[0050] S1. Weigh tungsten tailings sand, steel slag powder and slag powder according to weight proportion, mix them evenly to obtain dry material;
[0051] S2. Add water to the dry material obtained in step S1, mix well, and obtain tungsten tailings sand-steel slag powder solid waste synergistic paste filling material.
[0052] Step S1 of the present invention is to weigh tungsten tailings sand, steel slag powder and slag powder according to the weight ratio, mix them evenly, and obtain dry material. Specifically: weigh tungsten tailings sand, steel slag powder and slag powder according to the weight ratio, and mix them evenly by a mixer. The ash-sand ratio ((steel slag powder + slag powder): tungsten tailings sand) is 1: (5-7), which can be selected as 1: (5-5.5), 1: (5.5-6), 1: (6-6.5) or 1: (6.5-7), etc. Steel slag powder: slag powder = 1: (3-9), which can be selected as 1: (3-4), 1: (4-5), 1: (5-6), 1: (6-7), 1: (7-8) or 1: (8-9), etc. It is required that the amount of steel slag powder and the ash-sand ratio are positively correlated, that is, increasing the amount of steel slag powder in the paste filling material will increase the ash-sand ratio. .
[0053] In some embodiments of the present invention, the tungsten tailings are selected after screening, and the selected particle size range is 0.05-4mm, which can be 0.05-1mm, 1-1.5mm, 1.5-2mm, 2-2.5mm, 2.5-3mm, 3-3.5mm or 3.5-4mm, etc. The screening content of tungsten tailings is required to be less than 5% of <0.05mm and less than 5% of >4mm.
[0054] In some embodiments of the present invention, the steel slag powder is steel slag that is ground and then screened, and the selected particle size range is <45μm, which can be 1-10μm, 10-15μm, 15-25μm, 25-30μm, 30-35μm, 35-40μm or 40-45μm, etc. The screening content of tungsten tailings is required to be no more than 5% of <0.05mm and no more than 5% of >4mm.
[0055] In some embodiments of the present invention, the mixing in step S1 is performed by stirring with a stirrer for 2-3 minutes.
[0056] Step S2 of the present invention is to add water to the dry material obtained in step S1, mix them evenly, and obtain a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material. Specifically: water is added to the dry material obtained in step S1, and mixed evenly under the action of a stirrer to obtain a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material.
[0057] In some embodiments of the present invention, the mass ratio of dry material to water in step S2 is (1.8-2.7):1, which can be optionally (1.8-2):1, (2.2-2.5):1 or (2.5-2.7):1, etc.
[0058] In some embodiments of the present invention, the stirring time in step S2 is 3-5 min.
[0059] The third aspect of the present invention provides the use of tungsten tailings sand-steel slag powder solid waste synergistic paste filling material as a filling material.
[0060] In order to make the technical means, creative features, objectives and effects achieved by the present invention easier to understand, the present invention is described in detail below in conjunction with embodiments and drawings.
[0061] In the following examples, unless otherwise specified, all reaction raw materials are commercially available products.
[0062] Unless otherwise specified, the purity of each product in each embodiment of the present invention exceeds 98%.
[0063] Example 1
[0064] In the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material of the present embodiment, the particle size of the tungsten tailings sand is 0.04-4mm, the screening content of the particle size <0.05mm is ≤5%, and the screening content of the particle size >4mm is ≤5%; the moisture content is <12%, and the loss on ignition is <10%; the free calcium oxide content of the steel slag powder is <3%; the particle size range is <45μm, and the screening content of the particle size >45μm is ≤2%; the slag powder is S95 grade.
[0065] The preparation method of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material of this embodiment comprises the following steps:
[0066] S1 weighed 756kg of tungsten tailings, 38kg of steel slag powder and 121.6kg of slag powder, and stirred them in a mixer for 3min until they were evenly mixed to obtain dry material;
[0067] S2. Add 335 kg of water to the dry material obtained in step S1, use a mixer to stir for 4 minutes, mix evenly, and obtain a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material with a slurry concentration of 73%.
[0068] Example 2
[0069] The tungsten tailings sand, steel slag powder and slag powder in this embodiment are the same as those in Example 1.
[0070] The preparation method of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material of this embodiment comprises the following steps:
[0071] S1 weighed 756kg of tungsten tailings, 27kg of steel slag powder and 81kg of slag powder, and stirred them in a mixer for 3min until they were evenly mixed to obtain dry material;
[0072] S2. Add 320 kg of water to the dry material obtained in step S1, use a mixer to stir for 4 minutes, mix evenly, and obtain a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material with a slurry concentration of 73%.
[0073] Example 3
[0074] The tungsten tailings sand, steel slag powder and slag powder in this embodiment are the same as those in Example 1.
[0075] The preparation method of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material of this embodiment comprises the following steps:
[0076] S1 weighed 756kg of tungsten tailings, 15.1kg of steel slag powder and 136.1kg of slag powder, and stirred them in a mixer for 3min until they were evenly mixed to obtain dry material;
[0077] S2. Add 335 kg of water to the dry material obtained in step S1, use a mixer to stir for 4 minutes, mix evenly, and obtain a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material with a slurry concentration of 73%.
[0078] Example 4
[0079] The tungsten tailings sand, steel slag powder and slag powder in this embodiment are the same as those in Example 1.
[0080] The preparation method of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material of this embodiment comprises the following steps:
[0081] S1 weighed 756kg of tungsten tailings, 38kg of steel slag powder and 121.6kg of slag powder, and stirred them in a mixer for 3min until they were evenly mixed to obtain dry material;
[0082] S2. Add 488 kg of water to the dry material obtained in step S1, use a mixer to stir for 4 minutes, mix evenly, and obtain a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material with a slurry concentration of 65%.
[0083] Comparative Example 1
[0084] The tungsten tailings sand of Comparative Example 1 is the same as that of Example 1, and the cement comes from Anhui Conch Cement Co., Ltd.
[0085] The preparation method of the tungsten tailings sand-cement filling material of Comparative Example 1 comprises the following steps:
[0086] S1 weighed 756kg of tungsten tailings and 152kg of cement, stirred them in a mixer for 3min, and mixed them evenly to obtain dry material;
[0087] S2. Add 335 kg of water to the dry material obtained in step S1, stir with a mixer for 4 minutes, mix evenly, and obtain a tungsten tailings sand-cement filling material with a slurry concentration of 73%.
[0088] Comparative Example 2
[0089] The tungsten tailings, steel slag powder and slag powder of Comparative Example 2 are the same as those of Example 1.
[0090] The preparation method of the tungsten tailings sand-steel slag powder solid waste synergistic paste filling material of comparative example 2 comprises the following steps:
[0091] S1 weighed 756kg of tungsten tailings, 23.6kg of steel slag powder and 70.9kg of slag powder, and stirred them in a mixer for 3 minutes to obtain dry material;
[0092] S2. Add 315 kg of water to the dry material obtained in step S1, use a mixer to stir for 4 minutes, mix evenly, and obtain a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material with a slurry concentration of 73%.
[0093] Comparative Example 3
[0094] The tungsten tailings, steel slag powder and slag powder of Comparative Example 3 are the same as those of Example 1.
[0095] The preparation method of the tungsten tailings sand-steel slag powder solid waste synergistic paste filling material of comparative example 3 comprises the following steps:
[0096] S1 weighed 756kg of tungsten tailings, 60.5kg of steel slag powder and 90.7kg of slag powder, and stirred them in a mixer for 3 minutes to obtain dry material;
[0097] S2. Add 335 kg of water to the dry material obtained in step S1, use a mixer to stir for 4 minutes, mix evenly, and obtain a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material with a slurry concentration of 73%.
[0098] Comparative Example 4
[0099] The tungsten tailings, steel slag powder and slag powder of Comparative Example 4 are the same as those of Example 1.
[0100] The preparation method of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material of comparative example 4 comprises the following steps:
[0101] S1 weighed 756kg of tungsten tailings, 38kg of steel slag powder and 121.6kg of slag powder, and stirred them in a mixer for 3min until they were evenly mixed to obtain dry material;
[0102] S2. Add 226 kg of water to the dry material obtained in step S1, use a mixer to stir for 4 minutes, mix evenly, and obtain a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material with a slurry concentration of 80%.
[0103] Comparative Example 5
[0104] The tungsten tailings, steel slag powder and slag powder of Comparative Example 5 are the same as those of Example 1.
[0105] The preparation method of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material of comparative example 5 comprises the following steps:
[0106] S1 weighed 756kg of tungsten tailings, 38kg of steel slag powder and 121.6kg of slag powder, and stirred them in a mixer for 3min until they were evenly mixed to obtain dry material;
[0107] S2. Add 907 kg of water to the dry material obtained in step S1, use a mixer to stir for 4 minutes, mix evenly, and obtain a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material with a slurry concentration of 50%.
[0108] Performance Testing
[0109] According to the requirements of GB / T 50080 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures", the water bleeding rate, slump and setting time of Examples 1-4 and Comparative Examples 1-5 were tested, and the test results are shown in Table 1.
[0110] The uniaxial compressive strength of Examples 1-4 and Comparative Examples 1-5 was tested according to the requirements of JGJ / T 70 "Standard for Test Methods for Basic Properties of Building Mortar", and the linear shrinkage of Examples 1-4 and Comparative Examples 1-5 was tested according to the requirements of GB / T 39489 "Technical Specifications for Full Tailings Paste Filling", and the test results are shown in Table 1.
[0111] Table 1 Performance test of tungsten tailings sand-steel slag powder solid waste synergistic filling material
[0112] Serial number Water bleeding rate / % Slump / mm Coagulation time / h Uniaxial compressive strength / MPa Linear shrinkage / % Comparative Example 1 4.4 245 9.9 5.9 0.2 Comparative Example 2 2.9 217 11.6 0.4 3.1 Comparative Example 3 3.1 223 12.0 0.2 1.8 Comparative Example 4 0.9 114 9.5 3.7 2.2 Comparative Example 5 24.9 290 29.8 0.1 9.4 Example 1 3.5 235 12.9 2.8 3.7 Example 2 3.7 230 13.5 0.7 2.8 Example 3 3.1 233 12.7 3.6 1.9 Example 4 4.9 260 13.4 0.5 4.8
[0113] It can be seen from Comparative Example 1 and Example 1 that it is feasible to use steel slag powder and slag powder to replace cement as a binder for tungsten mine filling materials. Although its uniaxial compressive strength and slump are lower than those of cement binder, and its linear shrinkage is higher than that of cement binder, it can meet the requirements of GB / T 39489-2020, and its cost is lower than that of cement; it can be seen from Comparative Examples 2-5 and Example 1 that when the ash-sand ratio, that is, the ratio of binder (the sum of steel slag powder and slag powder) to tungsten tailings sand is lower than 1:7 or the ratio of steel slag powder: slag powder is greater than 1:3 or the slurry concentration is lower than 65%, the strength of the paste filling material is affected and reduced to varying degrees. In addition, when the slurry concentration is greater than 73%, the slump is low, which is not conducive to pipeline transportation and has poor workability. Especially when the slurry concentration is too low (less than 65%), the water permeability, slump, and linear shrinkage of the paste filling material are too large, the setting time is too long, and the uniaxial compressive strength is too low. It can be seen from Examples 1-4 that the tungsten tailings sand-steel slag powder solid waste synergistic filling material disclosed in the present invention, under the premise of meeting national standards, fully utilizes the cementing properties of steel slag powder, makes large amounts of use of tailings sand from tungsten mining, reduces the accumulation of tungsten tailings, and improves the comprehensive utilization rate of steel slag, slag, and tungsten tailings, which is conducive to circular and sustainable development and has significant economic benefits.
[0114] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A tungsten tailings sand-steel slag powder solid waste synergistic paste filling material, characterized in that: The tungsten tailings sand-steel slag powder solid waste collaborative paste filling material includes the following raw materials in parts by weight: 714-854 parts of tungsten tailings sand, 10-43 parts of steel slag powder, 76-154 parts of slag powder, and 300-551 parts of water.
2. The tungsten tailings sand-steel slag powder solid waste synergistic paste filling material according to claim 1, characterized in that: Includes any one or more of the following features: A1) The water seepage rate of the tungsten tailings sand-steel slag powder solid waste synergistic paste filling material is 1.5%-5%; A2) the slump of the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material is 200-260mm; A3) The setting time of the tungsten tailings sand-steel slag powder solid waste synergistic paste filling material is greater than 10h; A4) The uniaxial compressive strength of the tungsten tailings sand-steel slag powder solid waste synergistic paste filling material is 0.5-5Mpa; A5) The linear shrinkage rate of the tungsten tailings sand-steel slag powder solid waste synergistic paste filling material is less than 5%; A6) The slurry concentration of the tungsten tailings sand-steel slag powder solid waste and paste filling material is 65%-73%.
3. The tungsten tailings sand-steel slag powder solid waste synergistic paste filling material according to claim 1, characterized in that: Includes any one or more of the following features: B1) The mass ratio of the tungsten tailings to the steel slag powder and the slag powder is: 1: (5-7); B2) The mass ratio of the steel slag powder to the slag powder is 1:(3-9).
4. The tungsten tailings sand-steel slag powder solid waste synergistic paste filling material according to claim 1, characterized in that: Includes any one or more of the following features: C1) the particle size of the tungsten tailings is 0.05-4 mm; C2) the moisture content of the tungsten tailings is less than 12%; C3) the ignition loss of the tungsten tailings is less than 10%; C4) the free calcium oxide content of the steel slag powder is less than 3%; C5) The particle size range of the steel slag powder is <45 μm.
5. The tungsten tailings sand-steel slag powder solid waste synergistic paste filling material as claimed in claim 4, characterized in that: Also includes one or more of the following features: C11) The screening content of tungsten tailings with a particle size of <0.05mm is ≤5%; the screening content of tungsten tailings with a particle size of >4mm is ≤5%; C12) The screening content of steel slag powder with a particle size of >45μm is ≤2%.
6. A method for preparing a tungsten tailings sand-steel slag powder solid waste synergistic paste filling material as claimed in any one of claims 1 to 5, characterized in that: The steps include: S1. Weigh tungsten tailings sand, steel slag powder and slag powder according to weight proportion, mix them evenly to obtain dry material; S2. Add water to the dry material obtained in step S1, mix well, and obtain tungsten tailings sand-steel slag powder solid waste synergistic paste filling material.
7. The method for preparing the tungsten tailings sand-steel slag powder solid waste synergistic paste filling material according to claim 6, characterized in that: The mixing in step S1 is performed by stirring with a stirrer for 2-3 minutes.
8. The method for preparing the tungsten tailings sand-steel slag powder solid waste collaborative paste filling material according to claim 6, characterized in that: The mass ratio of dry material to water in step S2 is (1.8-2.7):
1.
9. The method for preparing the tungsten tailings sand-steel slag powder solid waste cooperative paste filling material according to claim 6, characterized in that: The mixing in step S2 is performed by using a stirrer, and the stirring time is 3-5 minutes.
10. Use of the tungsten tailings sand-steel slag powder solid waste synergistic paste filling material as described in any one of claims 1 to 9 as a filling material.