Gypsum composition, method for preparing gypsum mold from gypsum composition and application of gypsum mold
By using tartaric acid and polyvinylpyrrolidone as additives in gypsum molds to change their crystal form, the problem of insufficient strength and water absorption in existing gypsum molds is solved, and the balance between high strength and high water absorption is achieved, and the production process is simplified. Reduced costs and is suitable for mass production.
Patent Information
- Application Number
- CN202410992767.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing gypsum molds have shortcomings in terms of mechanical strength and water absorption, and it is difficult to meet the needs of high strength and water absorption at the same time. The production process is complex and costly, so it cannot meet the requirements of high-quality ceramic targets.
The composition of gypsum powder, tartaric acid and polyvinylpyrrolidone as additives is used to change the crystal form of the gypsum mold, and convert it from long strips to short blocks, which improves strength and retains high water absorption, while simplifying the production process and reducing costs. .
It realizes the high strength and high water absorption of gypsum molds, simplifies the production process, reduces costs, is suitable for large-scale mass production, and meets the high-quality needs of ceramic targets.
Smart Images

Figure CN118930207A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of target material manufacturing, and particularly relates to a gypsum composition, a method for preparing a gypsum mold with the gypsum composition, and application thereof. Background Art
[0002] With the continuous development of the application industry, higher requirements are put forward for the density of ceramic targets. Slurry injection molding has the advantages of high efficiency, wide adaptability, and high density of the molded body. It is especially suitable for large-sized ceramic target slurry molding. In order to obtain large-sized and high-density green blanks, it is necessary to use a larger slurry injection pressure to pour the slurry into a mold with many fine pores, which requires the mold to have higher strength. At the same time, the target industry has high requirements for the purity of the product, which requires that the slurry injection mold does not introduce new impurities during use.
[0003] Gypsum molds are widely used as molds in grouting molding due to their advantages such as low raw material cost and good processability. However, gypsum molds have low mechanical strength and low surface hardness. They are easily damaged during use, thereby introducing some impurities into the product, which cannot meet the demand for high-quality target products. The existing method for preparing gypsum molds is to mix α gypsum powder and β gypsum powder in a certain proportion. The specific gravity between α gypsum powder and β gypsum powder determines the strength and water absorption rate of gypsum. Often, the higher the strength of gypsum, the lower the water absorption rate, and the higher the water absorption rate, the lower the strength of gypsum. It is very difficult to obtain a gypsum mold with excellent water absorption and mechanical properties just by adjusting the ratio between α gypsum powder and β gypsum powder, so people turned their attention to additives.
[0004] Chinese patent CN103360012A discloses a gypsum mold for ceramic grouting and a preparation method thereof. The patent improves the strength and corrosion resistance of the gypsum mold by adding porous asphalt carbon. The disadvantage is that the foaming preparation of porous asphalt carbon needs to be carried out under high temperature and high pressure conditions. The mixing of gypsum powder and porous asphalt carbon and the pouring of gypsum slurry need to be carried out under vacuum conditions. The equipment environment conditions in the above production process are relatively harsh, and the conditions for large-scale mass production are not met, which increases the preparation cycle and production cost of the product. Chinese patent CN101204830A discloses an improved gypsum mold for ceramic grouting and a preparation method thereof. The patent improves the surface performance of the gypsum mold by coating a porous isolation layer containing solid particles and additive gel on the surface of the gypsum mold. The disadvantage is that the surface coating layer preparation and coating process of this method is complicated and not easy to mass produce. At the same time, this method improves the performance only by relying on the surface coating layer, and the performance of the gypsum mold itself has not changed. After a period of use, the loss of the coating layer will affect the use effect of the gypsum mold. Chinese patent CN108178601A discloses a gypsum mold for ceramic slip casting and its preparation method. The patent prepares a gypsum mold with high strength under vacuum conditions by adding inorganic additives, fiber reinforcements, and water retaining agents. The disadvantage is that this method enhances the strength of the gypsum mold by adding high-strength fibers, which is a physical reinforcement method. There will be gaps at the interface between the fiber and the gypsum matrix, which is a weak position in the system and is prone to water infiltration. Moreover, this method requires a more complex additive system and a more cumbersome production process to solve the negative effects, which increases the cycle and cost of gypsum mold production. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a gypsum composition, a method for preparing a gypsum mold using the gypsum composition and application thereof, wherein the prepared gypsum mold has both high strength and high water absorption.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a gypsum composition, which comprises, by weight:
[0008] 95-105 parts of gypsum powder, 0.05-3.2 parts of additives;
[0009] The additives include tartaric acid and polyvinyl pyrrolidone.
[0010] Preferably, the mass ratio of tartaric acid to polyvinyl pyrrolidone is 0.05-0.1:1-3.
[0011] Preferably, the gypsum powder includes α-gypsum powder and β-gypsum powder; the mass ratio of the α-gypsum powder to the β-gypsum powder is 30-50:50-70.
[0012] The present invention also provides a method for preparing a plaster mold using the gypsum composition, comprising the following steps:
[0013] The slurry obtained by mixing the gypsum composition described in the above technical solution with water is placed in a mold, and is sequentially subjected to static solidification, demoulding and drying to obtain a gypsum mold.
[0014] Preferably, the mass ratio of gypsum powder to water in the gypsum composition is 95-105:45-60.
[0015] Preferably, the standing and solidifying time is 30 to 120 minutes.
[0016] Preferably, the drying temperature is 35 to 60° C. and the drying time is 24 to 48 hours.
[0017] Preferably, the mixing is performed by adding the additives in the gypsum composition into water for a first stirring, and then adding the gypsum powder in the gypsum composition for a second stirring; the speeds of the first stirring and the second stirring are independently 50-100 rpm.
[0018] The present invention also provides the use of the gypsum mold prepared by the method described in the above scheme in the manufacture of target materials by grouting molding.
[0019] Preferably, the application is: mechanically processing the surface of the gypsum mold to obtain a gypsum mold for slip injection molding.
[0020] The present invention provides a gypsum composition, which comprises, by weight, 95 to 105 parts of gypsum powder and 0.05 to 3.2 parts of additives; the additives include tartaric acid and polyvinyl pyrrolidone. The additives used in the present invention mainly act on the crystallization process when the gypsum mold solidifies, change the crystal form of the gypsum mold after solidification, and convert the gypsum crystals from long strips to short blocks. Compared with the slender strips, the short blocks are not easy to break and have a more complete and regular crystal form, so that it has better strength. At the same time, the pore structure is not changed, the original porosity is retained, and the high water absorption rate is maintained, so that the gypsum mold has both the high strength and high water absorption rate required for grouting molding.
[0021] The present invention also provides a method for preparing a gypsum mold from a gypsum composition. The method has a simple production process, is easy to operate, does not need to be carried out under vacuum conditions, shortens the production cycle, reduces costs, and can easily achieve stable mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a scanning electron microscope image of the plaster mold prepared in Comparative Example 1;
[0023] Figure 2This is a scanning electron microscope image of the plaster mold prepared in Example 1. DETAILED DESCRIPTION
[0024] The present invention provides a gypsum composition, which comprises, by weight:
[0025] 95-105 parts of gypsum powder, 0.05-3.2 parts of additives;
[0026] The additives include tartaric acid and polyvinyl pyrrolidone.
[0027] Unless otherwise specified, the present invention has no special requirements on the sources of the raw materials used in the preparation, and commercially available products known to those skilled in the art can be used.
[0028] The gypsum composition provided by the present invention comprises 95 to 105 parts by mass of gypsum powder, preferably 95 to 100 parts, and most preferably 100 parts. In the present invention, the gypsum powder preferably comprises α gypsum powder and β gypsum powder; the mass ratio of the α gypsum powder to the β gypsum powder is preferably 30 to 50:50 to 70, and more preferably 40:60.
[0029] Based on 1 mass part of the gypsum powder, the gypsum composition provided by the present invention comprises 0.05 to 3.2 mass parts of additives, preferably 1.05 to 3.2 mass parts, and most preferably 2.1 mass parts. In the present invention, the tartaric acid is preferably DL-tartaric acid; the polyvinyl pyrrolidone (PVP) is preferably K30 type polyvinyl pyrrolidone (PVP-K30); the mass ratio of the tartaric acid to the polyvinyl pyrrolidone is preferably 0.05 to 0.1:1 to 3, more preferably 0.1:1 to 2, and most preferably 0.1:2.
[0030] The additive used in the present invention mainly acts on the crystallization process when the gypsum mold solidifies, changes the crystal form of the gypsum mold after solidification, and converts the gypsum crystals from long strips to short blocks. Compared with the long and thin strips, the short blocks are not easy to break and have a more complete and regular crystal form, so that they have better strength. At the same time, the pore structure is not changed, the original porosity is retained, and a high water absorption rate is maintained, so that the gypsum mold has both high strength and high water absorption rate required for grouting molding.
[0031] The present invention also provides a method for preparing a plaster mold using the gypsum composition, comprising the following steps:
[0032] The slurry obtained by mixing the gypsum composition described in the above technical solution with water is placed in a mold, and is sequentially subjected to static solidification, demoulding and drying to obtain a gypsum mold.
[0033] In the present invention, the mass ratio of gypsum powder to water in the gypsum composition is preferably 95-105:45-60, more preferably 95-100:50-55; the water is preferably pure water.
[0034] In the present invention, the mixing is preferably performed by adding the additives in the gypsum composition into water for a first stirring, and then adding the gypsum powder in the gypsum composition for a second stirring; the rates of the first stirring and the second stirring are independently preferably 50 to 100 rpm, more preferably 70 to 90 rpm; the time of the first stirring is preferably 5 to 10 min, more preferably 5 to 8 min; the time of the second stirring is preferably 5 to 30 min, more preferably 10 to 20 min.
[0035] In the present invention, the static solidification time is preferably 30 to 120 min, more preferably 40 to 80 min, and most preferably 60 min; the static solidification is preferably carried out at room temperature.
[0036] In the present invention, the drying temperature is preferably 35 to 60° C., more preferably 40 to 55° C.; the drying time is preferably 24 to 48 hours, more preferably 24 to 36 hours.
[0037] The preparation method provided by the present invention has a simple production process and is easy to operate, does not need to be carried out under vacuum conditions, shortens the production cycle, reduces costs, and can easily achieve stable mass production.
[0038] The present invention also provides the use of the gypsum mold described in the above technical solution or the gypsum mold prepared by the preparation method described in the above technical solution in slip casting to manufacture a target material.
[0039] In the present invention, the application is preferably: mechanically processing the surface of the gypsum mold to obtain a gypsum mold for grouting molding; the mechanical processing preferably includes milling, chamfering and trimming.
[0040] The present invention has no special limitation on the mechanical processing process. The gypsum mold can be processed into a gypsum mold for grouting molding with a desired shape and size by using a mechanical processing process well known in the art.
[0041] The technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention, but they should not be construed as limiting the protection scope of the present invention.
[0042] Example 1
[0043] The raw materials for preparing the gypsum mold provided by the present invention are composed of 100 parts of gypsum powder, 2.1 parts of additives, and 50 parts of water, wherein the gypsum powder is a mixture of α gypsum powder and β gypsum powder in a mass ratio of 40:60, and the additive comprises 0.1 parts of DL-tartaric acid and 302 parts of PVP-K;
[0044] The preparation method is as follows:
[0045] Add water into the mixer and stir at 60 rpm, then slowly pour in the additives and stir for 5 minutes;
[0046] Quickly pour the weighed gypsum powder into the mixer and continue stirring at 60 rpm for 10 min to obtain a slurry;
[0047] The slurry is poured into a pre-prepared mold, and the mold is demoulded after standing and solidifying at room temperature for 60 minutes, and then the demoulded mold is placed in a drying room and dried at 45° C. for 36 hours until constant weight is obtained to obtain a gypsum mold;
[0048] The gypsum mold is subjected to surface machining to obtain a gypsum mold for slip casting with a required shape and size.
[0049] Example 2
[0050] The difference from Example 1 is that the additives are 0.05 parts of DL-tartaric acid and 1 part of PVP-K30, and the rest of the contents are consistent with Example 1.
[0051] Example 3
[0052] The difference from Example 1 is that the additives are 0.05 parts of DL-tartaric acid and 2 parts of PVP-K30, and the rest of the contents are consistent with Example 1.
[0053] Example 4
[0054] The difference from Example 1 is that the additives are 0.05 parts of DL-tartaric acid and 3 parts of PVP-K30, and the rest of the contents are consistent with Example 1.
[0055] Example 5
[0056] The difference from Example 1 is that the additives are 0.1 parts of DL-tartaric acid and 1 part of PVP-K30, and the rest of the contents are consistent with Example 1.
[0057] Example 6
[0058] The difference from Example 1 is that the additives are 0.1 parts of DL-tartaric acid and 3 parts of PVP-K30, and the rest of the contents are consistent with Example 1.
[0059] Example 7
[0060] The difference from Example 1 is that the additives are 0.2 parts of DL-tartaric acid and 1 part of PVP-K30, and the rest of the contents are consistent with Example 1.
[0061] Example 8
[0062] The difference from Example 1 is that the additives are 0.2 parts of DL-tartaric acid and 2 parts of PVP-K30, and the rest of the contents are consistent with Example 1.
[0063] Example 9
[0064] The difference from Example 1 is that the additives are 0.2 parts of DL-tartaric acid and 3 parts of PVP-K30, and the rest of the contents are consistent with Example 1.
[0065] Comparative Example 1
[0066] The difference from Example 1 is that no additive is added, and the rest of the contents are consistent with Example 1.
[0067] Comparative Example 2
[0068] The difference from Example 1 is that the additive is 1 part of PVP-K30, and the rest of the contents are the same as Example 1.
[0069] Comparative Example 3
[0070] The difference from Example 1 is that the additive is 2 parts of PVP-K30, and the rest of the contents are the same as Example 1.
[0071] Comparative Example 4
[0072] The difference from Example 1 is that the additive is 3 parts of PVP-K30, and the rest of the content is consistent with Example 1.
[0073] Comparative Example 5
[0074] The difference from Example 1 is that the additive is 0.05 parts of DL-tartaric acid, and the rest of the contents are consistent with Example 1.
[0075] Comparative Example 6
[0076] The difference from Example 1 is that the additive is 0.1 parts of DL-tartaric acid, and the rest of the contents are the same as those in Example 1.
[0077] Comparative Example 7
[0078] The difference from Example 1 is that the additive is 0.2 parts of DL-tartaric acid, and the rest of the contents are consistent with Example 1.
[0079] Performance Testing
[0080] The absolute dry flexural strength, absolute dry compressive strength and water absorption of the gypsum molds prepared in Examples 1 to 9 and Comparative Examples 1 to 7 were tested, and the results are shown in Table 1.
[0081] The 2h wet flexural strength and absolute dry flexural strength were tested in accordance with the requirements of QB / T1640-2015 "Test Methods for Physical Properties of Gypsum Powder for Ceramic Moulds". Specifically, three test blocks were made to test their 2h wet flexural strength and absolute dry flexural strength. For the test piece for 2h wet flexural strength, the test piece was placed upright for 2h after demoulding (starting from the time when the gypsum powder came into contact with water) and then tested for its wet strength on a flexural testing machine; for the test piece for absolute dry flexural strength, the test piece was placed under conditions for 1d after demoulding and then dried in a (40±4℃) forced air drying oven until it was absolutely dry, then placed in a silica gel dryer and cooled to room temperature, and then tested for its absolute dry flexural strength on a flexural testing machine.
[0082] Test of absolute dry compressive strength: The compressive strength is measured on six half specimens obtained after the absolute dry flexural test. During the test, the specimen is placed in a compression fixture. The forming surface of the specimen should be perpendicular to the pressure surface. The pressure area is 40.0mm×62.5mm. The compression fixture and the specimen are placed on a compression testing machine to test its compressive strength.
[0083] Water absorption test: Take a 40mm×40mm×160mm test block, dry it in an oven at 45℃ until it is absolutely dry and weigh it (m0). Soak the test block in water for 48h until it is saturated with water. Take it out and wipe off excess water on the surface with a wet cloth and weigh it (m1). Calculate the water absorption according to the formula [(m1-m0) / m0]×100%.
[0084] Table 1 Performance test results of gypsum molds prepared in Examples 1 to 9 and Comparative Examples 1 to 7
[0085]
[0086]
[0087] As shown in Table 1, adding 0.1 parts of tartaric acid and 2 parts of PVP-K30 as additives in Example 1 is the best result of the present invention.
[0088] The above comparative examples 2 to 4 show that adding PVP-K30 alone as an additive can play a certain role in strengthening the gypsum mold and has basically no negative effect on the water absorption rate, but the strength increase is not obvious, and with the increase in the amount of PVP-K30, the strength is not further improved.
[0089] The addition of tartaric acid as an additive alone in Comparative Examples 5 to 7 has little effect on the absolute dry strength and water absorption rate of the gypsum mold, and mainly plays a certain retarding effect, increasing the solidification time of the gypsum mold.
[0090] From Examples 2 to 9, combined Figures 1-2 It shows that the main function of PVP-K30 is to affect the crystallization behavior of the gypsum mold during solidification.
[0091] Figure 1 This is a scanning electron microscope image of the plaster mold prepared in Comparative Example 1 without adding any additives. Figure 1 It can be seen that the main crystal form of the gypsum mold without any additives is long strip crystals.
[0092] Figure 2 This is a scanning electron microscope image of the plaster mold prepared in Example 1 with 0.1 parts of DL-tartaric acid and 2 parts of PVP-K30 added. Figure 2 It can be seen that the additive system affects the crystallization during the solidification process of gypsum. To a certain extent, it affects the orientation of the grain growth process, thereby changing the aspect ratio of the crystal form. The resulting crystal form is mainly short blocks, which have better strength than long strips. With the increase in the amount of DL-tartaric acid added, the solidification process of the gypsum mold is delayed, the time for PVP-K30 to take effect is extended, and the performance of the gypsum mold is further improved. However, with the further increase in the amount of DL-tartaric acid and PVP-K30, the upper limit of the amount of action has been reached, and the performance of the gypsum mold has hardly changed. Too many additives have adverse effects on the performance and cost of the product.
[0093] In summary, the present invention uses DL-tartaric acid combined with PVP-K30 as an additive for a gypsum mold, and can be used directly without special treatment of the additive. The additive system mainly acts on the crystallization process when the gypsum mold solidifies, changes the crystal form of the gypsum mold after solidification, and converts the gypsum crystal from a long strip to a short block. The prepared gypsum mold has the high strength and high water absorption required for grouting molding. At the same time, the production process of the method is simple and easy to operate, does not need to be carried out under vacuum conditions, and can easily achieve stable mass production.
[0094] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention rather than all the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A gypsum composition, characterized in that: In parts by mass, including: 95-105 parts of gypsum powder, 0.05-3.2 parts of additives; The additives include tartaric acid and polyvinyl pyrrolidone.
2. The gypsum composition according to claim 1, characterized in that The mass ratio of the tartaric acid to polyvinyl pyrrolidone is 0.05-0.1:1-3.
3. The gypsum composition according to claim 1, characterized in that The gypsum powder includes α gypsum powder and β gypsum powder; the mass ratio of the α gypsum powder to the β gypsum powder is 30-50:50-70.
4. A method for preparing a plaster mold using a gypsum composition, characterized in that: The following steps are involved: The slurry obtained by mixing the gypsum composition according to any one of claims 1 to 3 with water is placed in a mold, and the mixture is allowed to stand for solidification, demolded and dried in sequence to obtain a gypsum mold.
5. The method according to claim 4, characterized in that The mass ratio of gypsum powder to water in the gypsum composition is 95-105:45-60.
6. The method according to claim 4, characterized in that The standing and solidifying time is 30 to 120 minutes.
7. The method according to claim 4, characterized in that The drying temperature is 35 to 60° C.; the drying time is 24 to 48 hours.
8. The method according to claim 4, characterized in that The mixing comprises adding the additives in the gypsum composition into water for a first stirring, and then adding the gypsum powder in the gypsum composition for a second stirring; the speeds of the first stirring and the second stirring are independently 50-100 rpm.
9. Use of the gypsum mold prepared by the method according to any one of claims 4 to 8 in manufacturing target materials by slip casting.
10. The use according to claim 9, characterized in that: The application is: mechanically processing the surface of the gypsum mold to obtain a gypsum mold for slip injection molding.