Method for manufacturing autoclaved aerated concrete brick by using urban industrial solid waste

By using raw materials such as fly ash, red mud, desulfurization ash, blast furnace slag, cinder and waste gypsum to make autoclaved aerated concrete bricks, the problem that industrial solid waste treatment methods mainly rely on passive storage and landfill is solved. It realizes effective utilization of resources and environmental protection.

CN118930212AInactive Publication Date: 2024-11-12南京福盛新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411124676.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Industrial solid waste treatment methods mainly rely on passive storage, landfill, incineration and marine investment, resulting in waste of resources and environmental pollution.

Method used

The method of using urban industrial solid waste to make autoclaved aerated concrete bricks is adopted, and raw materials such as fly ash, red mud, desulfurization ash, blast furnace slag, cinder and waste gypsum are used to grind, stir, slurry, and slurry. Pouring and autoclaving processing, the autoclaved aerated concrete bricks are made to realize the recycling and reuse of industrial solid waste.

Benefits of technology

Effectively utilize industrial solid waste resources, reduce resource waste and environmental pollution, and provide an environmentally friendly treatment method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930212A_ABST
    Figure CN118930212A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of industrial solid waste recycling, and discloses a method for manufacturing autoclaved aerated concrete bricks by utilizing urban industrial solid waste, which comprises the following steps: selecting raw materials, namely selecting sand and fly ash, red mud, desulfurized fly ash, blast furnace slag, coal cinder and waste gypsum in the industrial solid waste as main raw materials, the sand, the blast furnace slag, the coal slag and the waste gypsum are put into ball milling equipment to be ground, and the blast furnace slag, the coal slag and the waste gypsum are ground into powder. Sand and fly ash, red mud, desulfurized fly ash, blast furnace slag, coal cinder and waste gypsum in industrial solid waste are selected as main raw materials, and the autoclaved aerated concrete brick is prepared according to the steps of raw material selection, metering and batching, mixing and stirring, slurry preparation, grouting and pouring, green brick preparation, green brick cutting and high-pressure steam curing. And part of industrial solid waste is recycled and reused, and industrial solid waste resources are effectively utilized while part of industrial solid waste is treated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of industrial solid waste recycling, and specifically relates to a method for manufacturing autoclaved aerated concrete bricks by utilizing urban industrial solid waste. Background Art

[0002] Industrial solid waste refers to solid waste generated during industrial production activities. It is various waste slag, dust and other waste discharged into the environment during the industrial production process. It can be divided into general industrial waste (such as blast furnace slag, steel slag, red mud, non-ferrous metal slag, fly ash, coal slag, sulfuric acid slag, waste gypsum, desulfurization ash, carbide slag, salt mud, etc.) and industrial hazardous solid waste, that is, hazardous solid waste.

[0003] Industrial solid waste is huge in quantity, diverse in types, and complex in composition, making it quite difficult to treat. Currently, only a limited number of industrial wastes are utilized, and the main method of treating industrial solid waste is still passive storage. Some harmful industrial solid wastes are disposed of by landfill, incineration, chemical conversion, microbial treatment and other methods. There is also a method of dumping solid waste into the ocean. Although they all have certain treatment effects, they cause waste of resources and have a greater impact on the environment.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] In order to solve the problem that the treatment method for industrial solid waste is still mainly passive storage, some harmful industrial solid waste is disposed of by landfill, incineration, chemical conversion, microbial treatment and other methods, and there is also a treatment method of throwing solid waste into the ocean. Although all of them have certain treatment effects, they cause waste of resources and have a greater impact on the environment. The basic concept of the technical solution adopted by the present invention is:

[0006] The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste comprises the following steps:

[0007] S1: Select raw materials, select sand and fly ash, red mud, desulfurization ash, blast furnace slag, coal slag, and waste gypsum from industrial solid waste as main raw materials, put sand, blast furnace slag, coal slag, and waste gypsum into a ball mill for grinding, and grind the blast furnace slag, coal slag, and waste gypsum into powder;

[0008] S2: Measuring and batching, adding fly ash, red mud, desulfurized ash, and powdered sand, blast furnace slag, coal slag, and waste gypsum into the mixing equipment in appropriate proportions;

[0009] S3: Mixing and stirring, adding an appropriate amount of water into the stirring equipment, and mixing and stirring the powdered raw materials such as sand, fly ash, red mud, desulfurization ash, blast furnace slag, coal slag and waste gypsum through the stirring equipment so that the raw materials can be fully mixed together;

[0010] S4: slurry preparation, adding appropriate amounts of expansion agent, regulator, and bubble stabilizer into the stirring device in sequence, and stirring at the same time to prepare a mixed slurry;

[0011] S5: Grouting and pouring, the prepared mixed slurry is evenly grouted into the brick mold, and the mixed material forms a green body after pouring and gasification, thereby preparing the green body of autoclaved aerated concrete brickwork;

[0012] S6: making brick blanks, placing the obtained brick blanks into a steaming chamber for processing, setting corresponding processing temperature and processing time, and making the brick blanks;

[0013] S7: Brick cutting: after the bricks are made, they are cut by corresponding cutting equipment to achieve the required product size;

[0014] S8: high-pressure steam curing. After the brick blanks are cut, they are placed in corresponding autoclaves for autoclaving. During the autoclaving, the temperature and time are controlled within the manufacturing range of autoclaved aerated concrete brickwork. After the autoclaving is completed, the brick blanks are taken out to obtain finished autoclaved aerated concrete brickwork products.

[0015] As a preferred embodiment of the present invention, in S1: the blast furnace slag, coal slag and waste gypsum account for 6%-10% of the total mass.

[0016] As a preferred embodiment of the present invention, in S1: the red mud accounts for 10%-14% of the total mass.

[0017] As a preferred embodiment of the present invention, in S1: the fly ash and desulfurization ash account for 3% of the total mass, and the sand accounts for 72% of the total mass.

[0018] As a preferred embodiment of the present invention, in S3: water accounts for 3% of the total mass, and water should be added gradually during the mixing and stirring process to ensure uniform stirring.

[0019] As a preferred embodiment of the present invention, in S3: the water used for mixing the raw materials is selected to be high-quality clean water with a certain fluidity and consistency.

[0020] As a preferred embodiment of the present invention, in S4: the expansion agent, regulator and bubble stabilizer account for 2% of the total mass, the expansion agent is an important factor determining the thermal insulation performance of autoclaved aerated concrete brickwork, and a composite expansion agent of aluminum powder-foaming agent is used.

[0021] As a preferred embodiment of the present invention, in S1: the sand is the aggregate in concrete and can enhance the strength of the blocks, and sand with uniform particle size and good quality is selected.

[0022] As a preferred embodiment of the present invention, in S1: the desulfurized ash is an important raw material for adjusting the activity of cement.

[0023] As a preferred embodiment of the present invention, in said S6: the obtained brick body is placed in a steam chamber for processing, the water is heated by steam, the expansion agent is decomposed to generate gas, and the mixed slurry is caused to rise.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention selects sand and fly ash, red mud, desulfurization ash, blast furnace slag, coal slag and waste gypsum from industrial solid waste as main raw materials, and prepares autoclaved aerated concrete brickwork according to the steps of selecting raw materials, metering and proportioning, mixing and stirring, slurry preparation, grouting and pouring, brick blank preparation, brick blank cutting and high-pressure steaming, so that part of the industrial solid waste is recycled and reused, and while part of the industrial solid waste is treated, the industrial solid waste resources are effectively utilized.

[0026] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In the attached picture:

[0028] Figure 1 This is an overall flow chart of the method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste;

[0029] Figure 2 The present invention is a flowchart of the production process of the method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The following embodiments are used to illustrate the present invention.

[0031] like Figure 1 to Figure 2 Shown

[0032] Embodiment 1

[0033] The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste comprises the following steps:

[0034] S1: Select raw materials, select sand and fly ash, red mud, desulfurization ash, blast furnace slag, coal slag, and waste gypsum from industrial solid waste as main raw materials, put sand, blast furnace slag, coal slag, and waste gypsum into a ball mill for grinding, and grind the blast furnace slag, coal slag, and waste gypsum into powder;

[0035] S2: Measuring and batching, adding fly ash, red mud, desulfurized ash, and powdered sand, blast furnace slag, coal slag, and waste gypsum into the mixing equipment in appropriate proportions;

[0036] S3: Mixing and stirring, adding an appropriate amount of water into the stirring equipment, and mixing and stirring the powdered raw materials such as sand, fly ash, red mud, desulfurization ash, blast furnace slag, coal slag and waste gypsum through the stirring equipment so that the raw materials can be fully mixed together;

[0037] S4: slurry preparation, adding appropriate amounts of expansion agent, regulator, and bubble stabilizer into the stirring device in sequence, and stirring at the same time to prepare a mixed slurry;

[0038] S5: Grouting and pouring, the prepared mixed slurry is evenly grouted into the brick mold, and the mixed material forms a green body after pouring and gasification, thereby preparing the green body of autoclaved aerated concrete brickwork;

[0039] S6: making brick blanks, placing the obtained brick blanks into a steaming chamber for processing, setting corresponding processing temperature and processing time, and making the brick blanks;

[0040] S7: Brick cutting: after the bricks are made, they are cut by corresponding cutting equipment to achieve the required product size;

[0041] S8: high-pressure steam curing. After the brick blanks are cut, they are placed in corresponding autoclaves for autoclaving. During the autoclaving, the temperature and time are controlled within the manufacturing range of autoclaved aerated concrete brickwork. After the autoclaving is completed, the brick blanks are taken out to obtain finished autoclaved aerated concrete brickwork products.

[0042] In a specific implementation manner, blast furnace slag, coal slag and waste gypsum account for 6% of the total mass, red mud accounts for 14% of the total mass, fly ash and desulfurization ash account for 3% of the total mass, and sand accounts for 72% of the total mass.

[0043] Further, in S3: water accounts for 3% of the total mass, and water should be gradually added during the mixing and stirring process to ensure uniform stirring;

[0044] In S3: The water used to mix the raw materials should be high-quality clean water with a certain fluidity and consistency;

[0045] In S4: the expansion agent, the regulator and the bubble stabilizer account for 2% of the total mass. The expansion agent is an important factor in determining the thermal insulation performance of autoclaved aerated concrete brickwork. A composite expansion agent of aluminum powder-foaming agent is used;

[0046] Further, in S1: sand is the aggregate in concrete, which can enhance the strength of the block, and sand with uniform particle size and good quality is selected;

[0047] In S1: Desulfurized ash is an important raw material for regulating cement activity;

[0048] In S6: the obtained brick body is placed in a steam chamber for processing, and the water is heated by steam to promote the decomposition of the expansion agent to generate gas, so that the mixed slurry rises.

[0049] Embodiment 2

[0050] The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste comprises the following steps:

[0051] S1: Select raw materials, select sand and fly ash, red mud, desulfurization ash, blast furnace slag, coal slag, and waste gypsum from industrial solid waste as main raw materials, put sand, blast furnace slag, coal slag, and waste gypsum into a ball mill for grinding, and grind the blast furnace slag, coal slag, and waste gypsum into powder;

[0052] S2: Measuring and batching, adding fly ash, red mud, desulfurized ash, and powdered sand, blast furnace slag, coal slag, and waste gypsum into the mixing equipment in appropriate proportions;

[0053] S3: Mixing and stirring, adding an appropriate amount of water into the stirring equipment, and mixing and stirring the powdered raw materials such as sand, fly ash, red mud, desulfurization ash, blast furnace slag, coal slag and waste gypsum through the stirring equipment so that the raw materials can be fully mixed together;

[0054] S4: slurry preparation, adding appropriate amounts of expansion agent, regulator, and bubble stabilizer into the stirring device in sequence, and stirring at the same time to prepare a mixed slurry;

[0055] S5: Grouting and pouring, the prepared mixed slurry is evenly grouted into the brick mold, and the mixed material forms a green body after pouring and gasification, thereby preparing the green body of autoclaved aerated concrete brickwork;

[0056] S6: making brick blanks, placing the obtained brick blanks into a steaming chamber for processing, setting corresponding processing temperature and processing time, and making the brick blanks;

[0057] S7: Brick cutting: after the bricks are made, they are cut by corresponding cutting equipment to achieve the required product size;

[0058] S8: high-pressure steam curing. After the brick blanks are cut, they are placed in corresponding autoclaves for autoclaving. During the autoclaving, the temperature and time are controlled within the manufacturing range of autoclaved aerated concrete brickwork. After the autoclaving is completed, the brick blanks are taken out to obtain finished autoclaved aerated concrete brickwork products.

[0059] In a specific implementation manner, blast furnace slag, coal slag and waste gypsum account for 7% of the total mass, red mud accounts for 13% of the total mass, fly ash and desulfurization ash account for 3% of the total mass, and sand accounts for 72% of the total mass.

[0060] Further, in S3: water accounts for 3% of the total mass, and water should be gradually added during the mixing and stirring process to ensure uniform stirring;

[0061] In S3: The water used to mix the raw materials should be high-quality clean water with a certain fluidity and consistency;

[0062] In S4: the expansion agent, the regulator and the bubble stabilizer account for 2% of the total mass. The expansion agent is an important factor in determining the thermal insulation performance of autoclaved aerated concrete brickwork. A composite expansion agent of aluminum powder-foaming agent is used;

[0063] Further, in S1: sand is the aggregate in concrete, which can enhance the strength of the block, and sand with uniform particle size and good quality is selected;

[0064] In S1: Desulfurized ash is an important raw material for regulating cement activity;

[0065] In S6: the obtained brick body is placed in a steam chamber for processing, and the water is heated by steam to promote the decomposition of the expansion agent to generate gas, so that the mixed slurry rises.

[0066] Embodiment 3

[0067] The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste comprises the following steps:

[0068] S1: Select raw materials, select sand and fly ash, red mud, desulfurization ash, blast furnace slag, coal slag, and waste gypsum from industrial solid waste as main raw materials, put sand, blast furnace slag, coal slag, and waste gypsum into a ball mill for grinding, and grind the blast furnace slag, coal slag, and waste gypsum into powder;

[0069] S2: Measuring and batching, adding fly ash, red mud, desulfurized ash, and powdered sand, blast furnace slag, coal slag, and waste gypsum into the mixing equipment in appropriate proportions;

[0070] S3: Mixing and stirring, adding an appropriate amount of water into the stirring equipment, and mixing and stirring the powdered raw materials such as sand, fly ash, red mud, desulfurization ash, blast furnace slag, coal slag and waste gypsum through the stirring equipment so that the raw materials can be fully mixed together;

[0071] S4: slurry preparation, adding appropriate amounts of expansion agent, regulator, and bubble stabilizer into the stirring device in sequence, and stirring at the same time to prepare a mixed slurry;

[0072] S5: Grouting and pouring, the prepared mixed slurry is evenly grouted into the brick mold, and the mixed material forms a green body after pouring and gasification, thereby preparing the green body of autoclaved aerated concrete brickwork;

[0073] S6: making brick blanks, placing the obtained brick blanks into a steaming chamber for processing, setting corresponding processing temperature and processing time, and making the brick blanks;

[0074] S7: Brick cutting: after the bricks are made, they are cut by corresponding cutting equipment to achieve the required product size;

[0075] S8: high-pressure steam curing. After the brick blanks are cut, they are placed in corresponding autoclaves for autoclaving. During the autoclaving, the temperature and time are controlled within the manufacturing range of autoclaved aerated concrete brickwork. After the autoclaving is completed, the brick blanks are taken out to obtain finished autoclaved aerated concrete brickwork products.

[0076] In a specific implementation manner, blast furnace slag, coal slag and waste gypsum account for 8% of the total mass, red mud accounts for 12% of the total mass, fly ash and desulfurization ash account for 3% of the total mass, and sand accounts for 72% of the total mass.

[0077] Further, in S3: water accounts for 3% of the total mass, and water should be gradually added during the mixing and stirring process to ensure uniform stirring;

[0078] In S3: The water used to mix the raw materials should be high-quality clean water with a certain fluidity and consistency;

[0079] In S4: the expansion agent, the regulator and the bubble stabilizer account for 2% of the total mass. The expansion agent is an important factor in determining the thermal insulation performance of autoclaved aerated concrete brickwork. A composite expansion agent of aluminum powder-foaming agent is used;

[0080] Further, in S1: sand is the aggregate in concrete, which can enhance the strength of the block, and sand with uniform particle size and good quality is selected;

[0081] In S1: Desulfurized ash is an important raw material for regulating cement activity;

[0082] In S6: the obtained brick body is placed in a steam chamber for processing, and the water is heated by steam to promote the decomposition of the expansion agent to generate gas, so that the mixed slurry rises.

[0083] Embodiment 4

[0084] The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste comprises the following steps:

[0085] S1: Select raw materials, select sand and fly ash, red mud, desulfurization ash, blast furnace slag, coal slag, and waste gypsum from industrial solid waste as main raw materials, put sand, blast furnace slag, coal slag, and waste gypsum into a ball mill for grinding, and grind the blast furnace slag, coal slag, and waste gypsum into powder;

[0086] S2: Measuring and batching, adding fly ash, red mud, desulfurized ash, and powdered sand, blast furnace slag, coal slag, and waste gypsum into the mixing equipment in appropriate proportions;

[0087] S3: Mixing and stirring, adding an appropriate amount of water into the stirring equipment, and mixing and stirring the powdered raw materials such as sand, fly ash, red mud, desulfurization ash, blast furnace slag, coal slag and waste gypsum through the stirring equipment so that the raw materials can be fully mixed together;

[0088] S4: slurry preparation, adding appropriate amounts of expansion agent, regulator, and bubble stabilizer into the stirring device in sequence, and stirring at the same time to prepare a mixed slurry;

[0089] S5: Grouting and pouring, the prepared mixed slurry is evenly grouted into the brick mold, and the mixed material forms a green body after pouring and gasification, thereby preparing the green body of autoclaved aerated concrete brickwork;

[0090] S6: making brick blanks, placing the obtained brick blanks into a steaming chamber for processing, setting corresponding processing temperature and processing time, and making the brick blanks;

[0091] S7: Brick cutting: after the bricks are made, they are cut by corresponding cutting equipment to achieve the required product size;

[0092] S8: high-pressure steam curing. After the brick blanks are cut, they are placed in corresponding autoclaves for autoclaving. During the autoclaving, the temperature and time are controlled within the manufacturing range of autoclaved aerated concrete brickwork. After the autoclaving is completed, the brick blanks are taken out to obtain finished autoclaved aerated concrete brickwork products.

[0093] In a specific implementation manner, blast furnace slag, coal ash and waste gypsum account for 9% of the total mass, red mud accounts for 11% of the total mass, fly ash and desulfurization ash account for 3% of the total mass, and sand accounts for 72% of the total mass.

[0094] Further, in S3: water accounts for 3% of the total mass, and water should be gradually added during the mixing and stirring process to ensure uniform stirring;

[0095] In S3: The water used to mix the raw materials should be high-quality clean water with a certain fluidity and consistency;

[0096] In S4: the expansion agent, the regulator and the bubble stabilizer account for 2% of the total mass. The expansion agent is an important factor in determining the thermal insulation performance of autoclaved aerated concrete brickwork. A composite expansion agent of aluminum powder-foaming agent is used;

[0097] Further, in S1: sand is the aggregate in concrete, which can enhance the strength of the block, and sand with uniform particle size and good quality is selected;

[0098] In S1: Desulfurized ash is an important raw material for regulating cement activity;

[0099] In S6: the obtained brick body is placed in a steam chamber for processing, and the water is heated by steam to promote the decomposition of the expansion agent to generate gas, so that the mixed slurry rises.

[0100] Embodiment 5

[0101] The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste comprises the following steps:

[0102] S1: Select raw materials, select sand and fly ash, red mud, desulfurization ash, blast furnace slag, coal slag, and waste gypsum from industrial solid waste as main raw materials, put sand, blast furnace slag, coal slag, and waste gypsum into a ball mill for grinding, and grind the blast furnace slag, coal slag, and waste gypsum into powder;

[0103] S2: Measuring and batching, adding fly ash, red mud, desulfurized ash, and powdered sand, blast furnace slag, coal slag, and waste gypsum into the mixing equipment in appropriate proportions;

[0104] S3: Mixing and stirring: Add an appropriate amount of water into the mixing equipment, and mix and stir the powdered raw materials such as sand, fly ash, red mud, desulfurization ash, blast furnace slag, coal slag and waste gypsum through the mixing equipment so that the raw materials can be fully mixed together;

[0105] S4: slurry preparation, adding appropriate amounts of expansion agent, regulator, and bubble stabilizer into the stirring device in sequence, and stirring at the same time to prepare a mixed slurry;

[0106] S5: Grouting and pouring, the prepared mixed slurry is evenly grouted into the brick mold, and the mixed material forms a green body after pouring and gasification, thereby preparing the green body of autoclaved aerated concrete brickwork;

[0107] S6: making brick blanks, placing the obtained brick blanks into a steaming chamber for processing, setting corresponding processing temperature and processing time, and making the brick blanks;

[0108] S7: Brick cutting: after the bricks are made, they are cut by corresponding cutting equipment to achieve the required product size;

[0109] S8: high-pressure steam curing. After the brick blanks are cut, they are placed in corresponding autoclaves for autoclaving. During the autoclaving, the temperature and time are controlled within the manufacturing range of autoclaved aerated concrete brickwork. After the autoclaving is completed, the brick blanks are taken out to obtain finished autoclaved aerated concrete brickwork products.

[0110] In a specific implementation manner, blast furnace slag, coal slag and waste gypsum account for 10% of the total mass, red mud accounts for 10% of the total mass, fly ash and desulfurization ash account for 3% of the total mass, and sand accounts for 72% of the total mass.

[0111] Further, in S3: water accounts for 3% of the total mass, and water should be gradually added during the mixing and stirring process to ensure uniform stirring;

[0112] In S3: The water used to mix the raw materials should be high-quality clean water with a certain fluidity and consistency;

[0113] In S4: the expansion agent, the regulator and the bubble stabilizer account for 2% of the total mass. The expansion agent is an important factor in determining the thermal insulation performance of autoclaved aerated concrete brickwork. A composite expansion agent of aluminum powder-foaming agent is used;

[0114] Further, in S1: sand is the aggregate in concrete, which can enhance the strength of the block, and sand with uniform particle size and good quality is selected;

[0115] In S1: Desulfurized ash is an important raw material for regulating cement activity;

[0116] In S6: the obtained brick body is placed in a steam chamber for processing, and the water is heated by steam to promote the decomposition of the expansion agent to generate gas, so that the mixed slurry rises.

Claims

1. A method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste. It is characterized in that The following steps are involved: S1: Select raw materials, select sand and fly ash, red mud, desulfurization ash, blast furnace slag, coal slag, and waste gypsum from industrial solid waste as main raw materials, put sand, blast furnace slag, coal slag, and waste gypsum into a ball mill for grinding, and grind the blast furnace slag, coal slag, and waste gypsum into powder; S2: Measuring and batching, adding fly ash, red mud, desulfurized ash, and powdered sand, blast furnace slag, coal slag, and waste gypsum into the mixing equipment in appropriate proportions; S3: Mixing and stirring, adding an appropriate amount of water into the stirring equipment, and mixing and stirring the powdered raw materials such as sand, fly ash, red mud, desulfurization ash, blast furnace slag, coal slag and waste gypsum through the stirring equipment so that the raw materials can be fully mixed together; S4: slurry preparation, adding appropriate amounts of expansion agent, regulator, and bubble stabilizer into the stirring device in sequence, and stirring at the same time to prepare a mixed slurry; S5: Grouting and pouring, the prepared mixed slurry is evenly grouted into the brick mold, and the mixed material forms a green body after pouring and gasification, thereby preparing the green body of autoclaved aerated concrete brickwork; S6: making brick blanks, placing the obtained brick blanks into a steaming chamber for processing, setting corresponding processing temperature and processing time, and making the brick blanks; S7: Brick cutting: after the bricks are made, they are cut by corresponding cutting equipment to achieve the required product size; S8: high-pressure steam curing. After the brick blanks are cut, they are placed in corresponding autoclaves for autoclaving. During the autoclaving, the temperature and time are controlled within the manufacturing range of autoclaved aerated concrete brickwork. After the autoclaving is completed, the brick blanks are taken out to obtain finished autoclaved aerated concrete brickwork products.

2. The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste according to claim 1, It is characterized in that In S1: the blast furnace slag, coal slag and waste gypsum account for 6%-10% of the total mass.

3. The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste according to claim 1, It is characterized in that In S1: the red mud accounts for 10%-14% of the total mass.

4. The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste according to claim 1, It is characterized in that In S1: the fly ash and desulfurized ash account for 3% of the total mass, and the sand accounts for 72% of the total mass.

5. The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste according to claim 1, It is characterized in that In S3: water accounts for 3% of the total mass, and water should be added gradually during the mixing and stirring process to ensure uniform stirring.

6. The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste according to claim 1, It is characterized in that In S3: the water used to mix the raw materials is selected to be high-quality clean water with a certain fluidity and consistency.

7. The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste according to claim 1, It is characterized in that In S4: the expansion agent, the regulator and the bubble stabilizer account for 2% of the total mass. The expansion agent is an important factor in determining the thermal insulation performance of autoclaved aerated concrete brickwork. A composite expansion agent of aluminum powder-foaming agent is used.

8. The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste according to claim 1, It is characterized in that In S1: the sand is the aggregate in concrete and can enhance the strength of the blocks. Sand with uniform particle size and good quality is selected.

9. The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste according to claim 1, It is characterized in that In S1: the desulfurized ash is an important raw material for adjusting the activity of cement.

10. The method for manufacturing autoclaved aerated concrete bricks using urban industrial solid waste according to claim 1, It is characterized in that In S6, the obtained brick body is placed in a steam chamber for processing, and the water is heated by steam to promote the decomposition of the expansion agent to generate gas, so that the mixed slurry rises.