Fixed-point light-transmitting ceramic rock plate with relief effect and manufacturing method of fixed-point light-transmitting ceramic rock plate

By using jade galactoplasmic blanks and water-retaining zirconium super white cosmetic soil in ceramic materials, combined with fixed-point donation of bonded ink and matte emulsion particle powder, the light transmittance and intensity balance of ceramic materials is solved. The above problems achieve the interweaving of jade transparency and light-shading effects, improving the artistic effect and production controllability of the product.

CN118930223AActive Publication Date: 2024-11-12JIANGXI WONDERFUL CERAMICS CO LTD +4
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411194288.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

When existing ceramic materials achieve fixed-point light transmission effect, they are difficult to be compatible with different powder materials, resulting in unbalanced strength of the blank, and problems such as broken blanks, broken blanks and cracked bricks during firing are prone to occur during production, and the jade quality cannot be achieved. The translucent feeling and light-shading effect interspersed.

Method used

Using jade galactoplasma combined with water-retaining zirconium super white cosmetic soil, the light-transmitting layer with high visible light perspective ratio is achieved through fixed-point donation of bonded ink and matte emulsion particle powder, combining bonded ink and matte The combination of emulsion particles powder can prepare fixed-point transparent ceramic rock slabs with relief effect.

Benefits of technology

The high visible light perspective ratio and jade translucency effect of the product are realized, solving the problems of light transmittance and intensity balance of traditional ceramic materials, and improving the artistic effect and production controllability of the product.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a fixed-point light-transmitting ceramic rock plate with an embossment effect and a preparation method of the fixed-point light-transmitting ceramic rock plate. The preparation method comprises the following steps: (1) pressing a jade semi-opacifying green body; (2) spraying water-retaining zirconium super-white engobe; (3) jet printing of bonding ink; (4) applying matte opacifying particle powder; (5) adsorbing and recovering the particle powder at the non-bonding ink position; (6) inkjet printing decoration; (7) applying protective glaze; and (8) high-temperature firing. The jade semi-opaque green body and the water-retaining zirconium ultra-white engobe are adopted to form a light-transmitting layer with a high visible light perspective ratio, and the bonding ink and the matte opaque particle powder are combined in the middle for fixed-point application, so that the embossment effect is achieved; and the jade transparent effect and the shading effect can be randomly positioned and interspersed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building ceramics, and particularly relates to a point-transmitting ceramic rock plate with relief effect and a manufacturing method thereof. Background Art

[0002] In recent years, with the continuous advancement of science and technology, the production technology of building ceramics has developed rapidly, various new processes and new formulas have been continuously applied, product development tends to be diversified, fashionable, environmentally friendly and healthy, and the decorative effect tends to be refined and personalized.

[0003] As a way of exporting Chinese culture throughout history, ceramics have integrated cultural elements into modern design to achieve the inheritance and continuation of culture. For example, the design of products such as gold inlaid jade, wood inlaid jade, stone inlaid jade, etc. not only integrates traditional craftsmanship with modern aesthetics, embodies the perfect combination of tradition and modernity, but also inherits and promotes local culture, becoming an important carrier for spreading culture.

[0004] CN101898891A discloses a semi-translucent ceramic material, a ceramic thin plate and a preparation method thereof. The method adopts a method of mixing a plurality of micro-powders, wherein the semi-translucent ceramic material is passed through a carved roller in cooperation with a belt to make the surface material freely fall onto a base material, and then is flattened by a rubber roller to realize staggered translucent areas and opaque areas, and achieve the effect of staggered translucent and opaque areas under light irradiation. This method of achieving the effect of staggered translucent and opaque areas by staggered fabrics, on the one hand, will keep the large pattern unchanged when the fabrics are laid, and can only make some small position changes locally, and cannot realize the random positioning matching of the surface decorative pattern and the translucent position; on the other hand, the semi-translucent ceramic material and the base material are two different powders, which are difficult to be compatible when combined. The mismatch of the two powders will lead to uneven strength of the blank, and the uniformity of the blank strength cannot be controlled. The blank is prone to breakage and cracking during the production process, and cracked bricks are also prone to occur during the firing process.

[0005] CN110845227A discloses a kind of positioned crystal flower translucent ceramic tile and its preparation method, which comprises inkjet printing a pattern on a translucent blank, applying crystal nucleus agent dry particles, and applying crystal flower dry particle glaze on the surface. Although this process can show the unique artistic beauty of the positioned crystal flower, the pattern will be blurred when inkjet is applied on the blank, and the subsequent application of crystal flower dry particles will further affect the color and transparency of the product. The overall decorative effect of the product is fuzzy and cannot achieve the transparency of jade.

[0006] The dramatic multi-color translucent three-dimensional effect ceramic rock slab and its manufacturing method disclosed in CN113896569A mainly prepare a variety of color translucent formulas for distribution, so as to achieve a three-dimensional texture effect from the surface to the bottom of the multi-color translucent blank. However, it is a fully transparent type and cannot achieve a fixed-point translucent effect. Summary of the invention

[0007] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a light-transmitting layer with a high visible light transmittance ratio formed by using a jade semi-opaque body + water-retaining zirconium-based ultra-white cosmetic clay, and combining the fixed-point application of bonding ink and matte opalescent granular powder in the middle to achieve a special artistic effect with a relief effect, and the jade-like transparent effect and the shading effect can be randomly positioned and interspersed. The product production is not difficult, and the controllable and operable fixed-point light-transmitting ceramic rock plate with a relief effect and a manufacturing method thereof are strong.

[0008] The technical solution of the present invention is a method for preparing the ceramic rock plate with relief effect and fixed-point light transmission, which is special in that it includes the following steps:

[0009] ⑴ Pressing jade semi-emulsified body;

[0010] ⑵ Water-retaining zirconium series ultra-white cosmetic soil;

[0011] ⑶ Printing adhesive ink;

[0012] (4) Apply matte opacifying granular powder;

[0013] ⑸ Adsorb and recover the particle powder in the area without bonding ink;

[0014] ⑹Inkjet printing decoration;

[0015] ⑺Apply protective glaze;

[0016] ⑻High temperature firing.

[0017] Preferably, the jade semi-opaque body described in step (1) is composed of the following components by weight: 10-25 parts of kaolin, 5-8 parts of black mud, 35-50 parts of glass frit, 2-5 parts of diopside, 6-10 parts of quartz powder, 10-15 parts of barium-based frit, 0.5-1 part of organic additives, and 1.0-2.0 parts of liquid dissolving agent.

[0018] Preferably, the kaolin is washed kaolin, the total content of iron, titanium and manganese impurities in the washed kaolin is controlled at 0.21-0.25%, the carbon content is controlled at 0.75-0.93%, and the dry strength is controlled at 3.5-4.2Mpa; under the conditions of a maximum firing temperature of 1200°C and a firing cycle of 70 minutes, the whiteness of the washed kaolin is 67°;

[0019] The black mud is a selected raw ore, the total content of iron, titanium and manganese impurities in the black mud is controlled at 0.47-0.52%, the carbon content is controlled at 1.35-1.48%, the drying strength is controlled at 5.2-7.1 MPa, and the whiteness of the black mud is 63° under the conditions of a maximum firing temperature of 1200°C and a firing cycle of 70 minutes;

[0020] The glass frit is a frit melted with waste glass as the main raw material, and the chemical composition of the glass frit is composed of the following components by weight percentage: SiO2 68.51%, Al2O3 13.82%, Fe2O30.10%, CaO 3.15%, MgO1.21%, K2O 9.68%, Na2O 1.38%, B2O3 2.15%;

[0021] The barium-based frit is a frit prepared with barium oxide as the base material, and the chemical composition of the barium-based frit is composed of the following components by weight percentage: SiO2 38.12%, Al2O3 15.46%, Fe2O3 0.01%, CaO 1.27%, MgO 2.17%, K2O 0.23%, Na2O 3.38%, BaO 39.36%;

[0022] The chemical composition of the diopside consists of the following components by weight: SiO2 56.49%, Al2O3 1.18%, Fe2O3 0.65%, CaO 23.24%, MgO 17.33%, K2O 0.06%, Na2O 0.41%, and LOI 0.64%.

[0023] As a preferred embodiment: the water-retaining zirconium-based ultra-white cosmetic clay described in step (2) is composed of the following components by weight: 30-40 parts of jade semi-emulsified body powder, 10-15 parts of ultrafine quartz powder, 10-20 parts of zircon white frit, 6-10 parts of calcined alumina powder, 1-3 parts of zirconium silicate, 10-15 parts of potassium feldspar, 5-8 parts of nepheline powder, 10-15 parts of ball clay, 2-3 parts of burnt talc, 0.5-1 parts of sodium tripolyphosphate + sodium hexametaphosphate, 0-0.5 parts of sodium carboxymethyl cellulose, and 0.5-1.2 parts of water retaining agent.

[0024] As a preferred embodiment: the ultrafine quartz powder, calcined alumina powder and zirconium silicate are industrial-grade raw materials, and the introduced fineness is 325 mesh sieve, and the median particle size is 30±5μm;

[0025] The potassium feldspar and nepheline powders have a fineness of 200 to 300 meshes;

[0026] The zirconium white frit is a frit containing zirconium and having a melting point of 900-1000° C. The chemical composition of the zirconium white frit is composed of the following components by weight percentage: SiO2 61.24%, Al2O3 10.15%, Fe2O3 0.14%, CaO 12.18%, MgO 3.05%, K2O 4.07%, Na2O 1.15%, ZrO2 5.44%, ZnO 2.13%, LOI 0.45%; its introduction fineness is 150-250 mesh;

[0027] The ball clay is a mixed clay mineral of montmorillonite, illite and kaolinite, and the chemical composition of the ball clay consists of the following components by weight percentage: SiO2 49.65%, Al2O3 34.92%, CaO0.14%, MgO 0.33%, K2O 2.02%, Na2O 0.10%, Fe2O3 1.51%, LOI 11.33%;

[0028] The water retaining agent is a hydrophilic water retaining agent, the main component of which is a polyol, which is a composite solution of one or more of propylene glycol, glycerol, polyethylene glycol, and 1,3-butylene glycol.

[0029] Preferably, the bonding ink in step (3) is composed of the following components in parts by weight: 5-7 parts of zirconium oxide, 18-25 parts of a binder, 65-70 parts of an alcohol ether solvent, and 3-5 parts of a dispersant.

[0030] Preferably, the bonding ink is further composed of the following components by weight: 7 parts of zirconium oxide, 20 parts of a binder, 70 parts of an alcohol ether solvent, and 3 parts of a dispersant.

[0031] Preferably, the matte opalescent granular powder in step (4) is composed of the following components by weight: 15 to 20 parts of barium-based frit, 10 to 20 parts of zirconium silicate, 30 to 50 parts of potassium feldspar powder, 10 to 15 parts of high-zinc low-temperature frit, 5 to 8 parts of strontium carbonate, 3 to 5 parts of kaolin, 0.5 to 1 part of sodium hexametaphosphate, and 0 to 0.3 part of sodium carboxymethyl cellulose.

[0032] Preferably, the high-zinc and low-temperature frit has a ZnO weight percentage content exceeding 10%, an initial melting temperature of 800-900°C, a high zinc content, and a low sintering temperature. The chemical composition of the high-zinc and low-temperature frit is composed of the following components by weight percentage: SiO2 60.5%, Al2O3 9.1%, CaO12.1%, MgO 2.2%, K2O 4.3%, Na2O 0.5%, and ZnO11.3%.

[0033] As a preferred embodiment, the jade semi-opaque body described in step (1) is further composed of the following components by weight: 17 parts of kaolin, 8 parts of black mud, 49 parts of glass frit, 4 parts of diopside, 6 parts of quartz powder, 11 parts of barium-based frit, 0.8 parts of organic additives, and 1 part of liquid dissolving agent; the chemical composition of the jade semi-opaque body is composed of the following components by weight percentage: SiO2 63.55%, Al2O3 17.65%, CaO 1.88%, MgO 2.23%, K2O 5.25%, Na2O 1.13%, Fe2O3 0.20%, BaO 4.32%, LOI 3.79%; the preparation method of the jade semi-emulsified body powder is as follows: the jade semi-emulsified body formula raw materials are subjected to graded ball milling, and after the ball milling reaches the qualified fineness, the mud is placed in the high-level pool for uniform stirring, and the mud control parameters are as follows: the fineness is 1.88% of the 325 mesh residue, the water content is 36.8%, the mud Engler viscosity is 83S, the D50 particle size is 7.79μm, and the spray drying and granulation are carried out using natural gas as the heat source to obtain the jade semi-emulsified body powder.

[0034] As a preferred embodiment: the water-retaining zirconium-based ultra-white cosmetic soil described in step (2) is further composed of the following components by weight: 35 parts of jade semi-emulsified body powder, 12 parts of ultrafine quartz powder, 15 parts of zircon white frit, 6 parts of calcined alumina powder, 3 parts of zirconium silicate, 10 parts of potassium feldspar, 7 parts of nepheline powder, 10 parts of ball clay, 2 parts of burnt talc, 0.7 parts of sodium tripolyphosphate + sodium hexametaphosphate, 0.3 parts of sodium carboxymethyl cellulose, and 0.8 parts of water retaining agent; the chemical composition of the water-retaining zirconium-based ultra-white cosmetic soil is composed of the following components by weight percentage: SiO2 62.47%, Al2O3 22.95%, Fe2O3 0.15%, CaO 1.76%, MgO2.13%, K2O4.34%, Na2O 1.68%, ZrO2 2.92%, BaO 1.60%; the preparation method of the water-retaining zirconium-based ultra-white cosmetic soil is as follows: according to the formula of the water-retaining zirconium-based ultra-white cosmetic soil, jade semi-emulsified green body powder, ultrafine quartz powder, zirconium white frit, calcined alumina powder, zirconium silicate, potassium feldspar, nepheline powder, ball clay, burned talc, sodium tripolyphosphate, sodium hexamethaphosphate, and sodium carboxymethyl cellulose are placed in a ball mill, and then 40 parts of water are added, and the ball mill is milled to a fineness of 0.4-0.7% after the residue on a 325-mesh sieve is removed, and after the removal of the slurry, a water-retaining agent is added to the slurry and stirred evenly, and then the slurry is deironed to control the iron content in the cosmetic soil slurry to be 0.13-0.15%.

[0035] As a preference: the matte opacifying granular powder described in step (4) is further composed of the following components by weight: 15 parts of barium-based frit, 20 parts of zirconium silicate, 40 parts of potassium feldspar powder, 15 parts of high-zinc low-temperature frit, 5 parts of strontium carbonate, 5 parts of kaolin, 0.78 parts of sodium hexametaphosphate, and 0.21 parts of sodium carboxymethyl cellulose. The chemical composition of the matte opacifying granular powder is composed of the following components by weight percentage: SiO2 56.68%, Al2O3 14.12%, CaO 1.91%, MgO 0.37%, K2O 4.82%, Na2O1.33%, Fe2O3 0.12%, ZnO 1.73%, ZrO2 13.08%, SrO 3.60%, LOI 2.24%; the preparation method of the matte opalescent granular powder is as follows: weigh the matte opalescent granular powder according to the formula and put it into a ball mill, then add 40 parts of water, ball mill to a fineness of 0.15-0.35% of the residue on a 325-mesh sieve, and then adjust the glaze slurry to an Engler viscosity of 42S and a specific gravity of 1.82-1.91, and then use a spray dryer to make the slurry into powder particles, the moisture content of the powder particles is 1.8%, and the bulk density is 0.96g / cm 3 , and then put the obtained powder particles into a kiln for firing. The maximum firing temperature is controlled at 950-1020°C and the firing cycle is 6 hours to obtain a matte opacified granular powder product.

[0036] As a preference: the protective glaze described in step (7) is selected and adjusted according to the gloss and texture of product development, and is preferably a matte protective glaze.

[0037] Another technical solution of the present invention is the ceramic rock slab with relief effect and point-to-point light transmission, which is special in that it is prepared by the preparation method of the ceramic rock slab with relief effect and point-to-point light transmission as described in any one of claims 1 to 9 and 13.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] (1) Glass frit is added to the jade-like semi-opaque green body formula of the present invention. The glass frit has the characteristics of low melting temperature and wide sintering temperature range, which can not only improve the whiteness of the ceramic green body, but also form potassium barium feldspar and calcium feldspar with the barium-based frit at a relatively low temperature, thereby increasing the light transmittance of the green body.

[0040] (2) Barium-based frit is added to the jade-like semi-opaque green body formula of the present invention. During the firing process, the barium-based frit forms barium cryolite with a refractive index close to that of the glass phase, which reduces the glass phase in the green body while increasing the crystalline phase content in the green body, which is beneficial to improving the high-temperature sintering performance of the ceramic green body, reducing the loss of light in the ceramic green body, and improving the light transmittance of the green body. This solves the problem that traditional light-transmitting bricks add barium carbonate raw materials to improve the light transmittance, and then introduce carbon elements, resulting in excessive loss of components in the green body during burning, leading to a black core in the green body.

[0041] ⑶ The water-retaining zirconium-based ultra-white cosmetic clay of the present invention is prepared with jade-like semi-emulsified body powder as the basic raw material, and has better body-glaze matching and high whiteness, which is beneficial to the coloring of inkjet ink, can prevent the bonding ink printed in the next process from quickly penetrating into the body, is beneficial to the subsequent adhesion of granular powder, and ensures the bonding process effect of the subsequent process.

[0042] (4) The organic material in the bonding ink of the present invention is zirconium oxide. Under high-temperature firing conditions, the zirconium oxide can react deeply with the matte opacifying particle powder to generate a zirconium-based glaze layer with obvious opacifying effect.

[0043] (5) The matte opacified granular powder of the present invention is made by a light calcination process, and the particles tend to be spherical. Compared with traditional frit dry particles, the powder made by the light calcination process has better fluidity.

[0044] (6) The matte opacifying granular powder of the present invention has a high initial melting point and good reaction activity. It is easy to fully react with the zirconium oxide in the bonding ink under high-temperature firing conditions to generate a zirconium-based glaze layer with obvious opacifying effect, that is, the product is an opacifying glaze layer at the position where the matte opacifying granular powder is adhered after firing. The bonding ink design file can be adjusted according to the product development and design requirements. The layout of the bonding ink quantity is controlled by the file. The position without bonding ink will not be adhered to the matte opacifying granular powder. When the thickness of the blank is 9 mm, the visible light transmittance of the blank + glaze layer at this position after firing is 5.5%. The bonded matte opacifying granular powder at the position where the grayscale of the bonding ink printing file is 100% is ≥500g / m 2 The visible light transmittance of the body + glaze layer at this position is 0, thereby achieving a special artistic effect of interweaving jade-like translucent effect and shading effect. When jade-like files are used at the light-transmitting effect position, unique effects such as inlaid jade can be formed after firing. DETAILED DESCRIPTION

[0045] The present invention will be further described in detail below in conjunction with embodiments:

[0046] The method for preparing a point-transmitting ceramic rock plate with a relief effect is as follows:

[0047] ⑴ Pressing jade semi-emulsified body,

[0048] ⑵Water-retaining zirconium series ultra-white cosmetic soil,

[0049] ⑶ Printing adhesive ink,

[0050] ⑷Apply matte opacifying granular powder,

[0051] ⑸ Adsorb and recover the particle powder where there is no adhesion to the ink,

[0052] ⑹Inkjet printing decoration,

[0053] ⑺Apply protective glaze,

[0054] ⑻High temperature firing.

[0055] Wherein: the jade semi-emulsified body described in step (1) is a green body whose whiteness after firing is controlled at 70-73°, and when the thickness is 6 mm, the visible light transmittance ratio is 19.3%; when the thickness is 9 mm, the visible light transmittance ratio is 6.3% of the high-white body, and the corresponding powder control parameters are: moisture 4.7-6.0%, bulk density 0.92, strength before drying 0.71 MPa, and strength after drying 6.3 MPa.

[0056] The jade semi-opaque body formula is composed of the following components by weight: 17 parts of kaolin, 8 parts of black mud, 49 parts of glass frit, 4 parts of diopside, 6 parts of quartz powder, 11 parts of barium-based frit, 0.8 parts of organic additives, and 1 part of liquid dissolving agent; the chemical composition of the jade semi-opaque body is composed of the following components by weight percentage: SiO2 63.55%, Al2O3 17.65%, CaO1.88%, MgO 2.23%, K2O 5.25%, Na2O 1.13%, Fe2O3 0.20%, BaO 4.32%, and LOI 3.79%;

[0057] The kaolin is water-washed kaolin. To ensure the whiteness of the green body, the total content of impurities such as iron, titanium, and manganese in the water-washed kaolin is controlled at 0.21-0.25%, the carbon content is controlled at 0.75-0.93%, and the dry strength is controlled at 3.5-4.2 MPa. Under the conditions of a maximum firing temperature of 1200° C. and a firing cycle of 70 minutes, the whiteness of the water-washed kaolin is 67°.

[0058] The black mud is a selected ore. To ensure the whiteness of the green body, the total content of impurities such as iron, titanium, and manganese in the black mud is controlled at 0.47-0.52%, the carbon content is controlled at 1.35-1.48%, and the dry strength is controlled at 5.2-7.1 MPa. Under the conditions of a maximum firing temperature of 1200°C and a firing cycle of 70 minutes, the whiteness of the black mud is 63°. The black mud has the advantages of high dry strength, high viscosity, good bonding performance, convenient processing, and stable quality.

[0059] The glass frit is a frit melted with waste glass as the main raw material. The chemical composition of the glass frit consists of the following components by weight: SiO2 68.51%, Al2O3 13.82%, Fe2O3 0.10%, CaO 3.15%, MgO 1.21%, K2O 9.68%, Na2O 1.38%, and B2O3 2.15%.

[0060] Special note: Glass frit is added to the jade semi-opaque body formula. Taking advantage of the glass frit's low melting temperature and wide sintering temperature range, it can not only improve the whiteness of the ceramic body, but also form potassium barium feldspar and calcium feldspar with the barium-based frit at a lower temperature, thereby increasing the body's light transmittance.

[0061] The barium-based frit is a frit prepared with barium oxide as the base material, and the chemical composition of the barium-based frit is as follows by weight: SiO2 38.12%, Al2O3 15.46%, Fe2O3 0.01%, CaO 1.27%, MgO 2.17%, K2O 0.23%, Na2O 3.38%, and BaO 39.36%.

[0062] Special note: Barium-based frit is added to the formula of the jade semi-emulsified body. During the firing process, the barium-based frit forms barium cryolite with a refractive index close to that of the glass phase, which reduces the glass phase in the body and increases the crystalline phase content in the body. This is beneficial to improving the high-temperature sintering performance of the ceramic body, reducing the loss of light in the ceramic body, and improving the light transmittance of the body. It solves the problem that traditional translucent bricks add barium carbonate raw materials to improve the light transmittance, and then introduce carbon elements, causing excessive loss of components in the body due to burning, resulting in a black core in the body.

[0063] The chemical composition of the diopside is as follows by weight: SiO2 56.49%, Al2O3 1.18%, Fe2O3 0.65%, CaO 23.24%, MgO 17.33%, K2O 0.06%, Na2O 0.41%, and LOI 0.64%.

[0064] Special note: The characteristic of diopside crystals is that they are conducive to fast firing. Calcium and magnesium elements exist in their components. At the firing temperature, a rapidly soluble calcium-containing glass phase can be generated, and its viscosity decreases sharply with increasing temperature. Using a small amount can avoid the problem of a narrow firing range of the formula.

[0065] The organic additive is mainly a green body toughening and strengthening material, and its main component is one or a combination of modified lignin, polyvinyl alcohol, polyacrylamide, and sodium carboxymethyl cellulose.

[0066] The method for preparing jade semi-emulsified green body powder comprises: subjecting jade semi-emulsified green body formula raw materials to graded ball milling, after ball milling to a qualified fineness, placing mud in a high-level pool for uniform stirring, wherein mud control parameters are: fineness of 325-mesh sieve residue of 1.88%, water content of 36.8%, mud Engler viscosity of 83S, D50 particle size of 7.79 μm, and spray drying and granulation with natural gas as a heat source to obtain jade semi-emulsified green body powder.

[0067] Wherein: the water-retaining zirconium-based ultra-white cosmetic soil described in step (2) is a zirconium-based ultra-white cosmetic soil with high whiteness, favorable for inkjet ink coloring, and water-retaining properties obtained by adjusting jade semi-emulsified body powder as the basic raw material, and the glazing method is adopted, the glazing specific gravity is 1.79-1.85, and the glazing amount is 485-490 g / m 2 .

[0068] The water-retaining zirconium-based ultra-white cosmetic soil is composed of the following components by weight: 35 parts of jade semi-emulsified green body powder, 12 parts of ultrafine quartz powder, 15 parts of zircon white frit, 6 parts of calcined alumina powder, 3 parts of zirconium silicate, 10 parts of potassium feldspar, 7 parts of nepheline powder, 10 parts of ball clay, 2 parts of burnt talc, 0.7 parts of sodium tripolyphosphate + sodium hexametaphosphate, 0.3 parts of sodium carboxymethyl cellulose, and 0.8 parts of water-retaining agent; the chemical composition of the water-retaining zirconium-based ultra-white cosmetic soil is composed of the following components by weight percentage: SiO2 62.47%, Al2O3 22.95%, Fe2O3 0.15%, CaO 1.76%, MgO 2.13%, K2O 4.34%, Na2O 1.68%, ZrO2 2.92%, and BaO 1.60%.

[0069] Special note: The jade semi-emulsified body powder in the formula of water-retaining zirconium-based ultra-white cosmetic clay is not limited to fixed selected materials. In terms of technical indicators, as long as the powder is fired at a maximum temperature of 1200°C and a firing cycle of 70 minutes, the whiteness of the single material is between 70 and 73°, and when the thickness is 6 mm, the visible light transmittance is not less than 19.3%, the iron content is less than 0.15%, and the aluminum oxide content is in the range of 19 to 23%, it can be equivalent to replacing the jade semi-emulsified body powder.

[0070] The ultrafine quartz powder, calcined alumina powder and zirconium silicate are industrial-grade raw materials, and the introduced fineness is 325 mesh sieve, and the median particle size is 30±5μm. The calcined alumina powder is made of industrial aluminum hydroxide as raw material, and is calcined at a high temperature of more than 1280°C. The obtained calcined alumina powder is mainly α-A12O3 crystal type, has good activity, and has a high degree of participation in the reaction in the glaze.

[0071] The potassium feldspar and nepheline powders have a fineness of 250-280 meshes;

[0072] The zirconium white frit is a frit containing zirconium and having an initial melting temperature of 900-1000° C. The chemical composition of the zirconium white frit is as follows by weight: SiO2 61.24%, Al2O3 10.15%, Fe2O3 0.14%, CaO 12.18%, MgO 3.05%, K2O4.07%, Na2O 1.15%, ZrO2 5.44%, ZnO 2.13%, LOI 0.45%, and the introduced fineness is 180-220 meshes.

[0073] The ball clay is a mixed clay mineral of montmorillonite, illite and kaolinite, and the chemical composition of the ball clay is as follows by weight: SiO2 49.65%, Al2O3 34.92%, CaO 0.14%, MgO 0.33%, K2O 2.02%, Na2O 0.10%, Fe2O3 1.51%, and LOI 11.33%.

[0074] Special note: Montmorillonite has strong water absorption and expansion properties and can form a colloidal structure. Illite can also exhibit colloidal properties and both have certain water retention properties.

[0075] The water retaining agent is a hydrophilic water retaining agent, the main component of which is a polyol, which is a composite solution of one or more of propylene glycol, glycerol, polyethylene glycol and 1,3-butylene glycol.

[0076] The preparation method of the water-retaining zirconium-based ultra-white cosmetic soil comprises: placing jade semi-emulsified green body powder, ultra-fine quartz powder, zirconium white frit, calcined alumina powder, zirconium silicate, potassium feldspar, nepheline powder, ball clay, calcined talc, sodium tripolyphosphate, sodium hexamethaphosphate and sodium carboxymethyl cellulose into a ball mill according to the formula of the water-retaining zirconium-based ultra-white cosmetic soil, adding 40 parts of water, ball milling to a fineness of 0.5-0.6% on a 325-mesh sieve, discharging slurry, adding a water-retaining agent into the slurry after discharging slurry, stirring evenly, and then removing iron from the slurry to control the iron content in the cosmetic soil slurry to be 0.13%.

[0077] Wherein: the bonding ink described in step (3) is printed by inkjet printing, using dual-channel inkjet, and when the inkjet design adopts 100% grayscale, the total ink volume of the dual-channel glue ink inkjet printing is 125g / m 2 .

[0078] The bonding ink consists of the following components by weight: 7 parts of zirconium oxide, 20 parts of a binder, 70 parts of an alcohol ether solvent, and 3 parts of a dispersant.

[0079] The adhesive is mainly a hot-melt adhesive, which is an adhesive material with vinyl resin as the main component.

[0080] Among them: Matt opacifying granular powder adopts light burning process, and the thickness of application is ≥500g / m 2 The granular powder has a visible light transmittance of 0 after firing.

[0081] The matte opalescent granular powder described in step (4) is composed of the following components by weight: 15 parts of barium-based frit, 20 parts of zirconium silicate, 40 parts of potassium feldspar powder, 15 parts of high-zinc low-temperature frit, 5 parts of strontium carbonate, 5 parts of kaolin, 0.78 parts of sodium hexametaphosphate, and 0.21 parts of sodium carboxymethyl cellulose.

[0082] The chemical composition of the matte opacifying granular powder consists of the following components by weight percentage: SiO2 56.68%, Al2O3 14.12%, CaO 1.91%, MgO 0.37%, K2O 4.82%, Na2O 1.33%, Fe2O3 0.12%, ZnO 1.73%, ZrO2 13.08%, SrO 3.60%, and LOI 2.24%.

[0083] The preparation method of the matte opalescent granular powder is as follows: weigh the matte opalescent granular powder according to the formula and put it into a ball mill, then add 40 parts of water, ball mill until the fineness is 0.28-0.32% of the residue on a 325-mesh sieve, and then adjust the glaze slurry to an Engler viscosity of 42S and a specific gravity of 1.85, and then use a spray dryer to make the slurry into powder particles, wherein the moisture content of the powder particles is 1.8% and the bulk density is 0.96g / cm 3 , and then put the obtained powder particles into a kiln for firing. The maximum firing temperature is controlled at 980°C and the firing cycle is 6 hours to obtain a matte opalescent granular powder product.

[0084] The high-zinc low-temperature frit is a frit with a ZnO weight percentage exceeding 10%, an initial melting temperature of 800-900° C., a high zinc content, and a low sintering temperature. The chemical composition of the high-zinc low-temperature frit is as follows by weight percentage: SiO2 60.5%, Al2O3 9.1%, CaO 12.1%, MgO 2.2%, K2O 4.3%, Na2O 0.5%, and ZnO 11.3%;

[0085] The protective glaze described in step (7) is selected and adjusted according to the gloss and texture of the product development, and is preferably a matte spray protective glaze.

[0086] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should fall within the scope of the claims of the present invention.

Claims

1. A method for preparing a ceramic rock plate with relief effect and fixed-point light transmission, characterized in that: The following steps are involved: ⑴ Pressing jade semi-emulsified body; ⑵ Water-retaining zirconium series ultra-white cosmetic soil; ⑶ Printing adhesive ink; (4) Apply matte opacifying granular powder; ⑸ Adsorb and recover the particle powder in the area without bonding ink; ⑹Inkjet printing decoration; ⑺Apply protective glaze; ⑻High temperature firing.

2. The method for preparing the point-transmitting ceramic rock plate with relief effect according to claim 1, characterized in that: The jade semi-emulsified body described in step (1) is composed of the following components by weight: 10 to 25 parts of kaolin, 5 to 8 parts of black mud, 35 to 50 parts of glass frit, 2 to 5 parts of diopside, 6 to 10 parts of quartz powder, 10 to 15 parts of barium-based frit, 0.5 to 1 part of organic additives, and 1.0 to 2.0 parts of liquid degumming agent.

3. The method for preparing the point-transmitting ceramic rock plate with relief effect according to claim 2, characterized in that: The kaolin is washed kaolin, the total content of iron, titanium and manganese impurities in the washed kaolin is controlled at 0.21-0.25%, the carbon content is controlled at 0.75-0.93%, and the dry strength is controlled at 3.5-4.2Mpa; under the conditions of a maximum firing temperature of 1200°C and a firing cycle of 70 minutes, the whiteness of the washed kaolin is 67°; The black mud is a selected raw ore, the total content of iron, titanium and manganese impurities in the black mud is controlled at 0.47-0.52%, the carbon content is controlled at 1.35-1.48%, the drying strength is controlled at 5.2-7.1 MPa, and the whiteness of the black mud is 63° under the conditions of a maximum firing temperature of 1200°C and a firing cycle of 70 minutes; The glass frit is a frit melted with waste glass as the main raw material, and the chemical composition of the glass frit is composed of the following components by weight percentage: SiO2 68.51%, Al2O3 13.82%, Fe2O3 0.10%, CaO 3.15%, MgO1.21%, K2O 9.68%, Na2O 1.38%, B2O3 2.15%; The barium-based frit is a frit prepared from barium oxide as a base material, and the chemical composition of the barium-based frit is composed of the following components by weight percentage: SiO2 38.12%, Al2O3 15.46%, Fe2O3 0.01%, CaO1.27%, MgO 2.17%, K2O0.23%, Na2O 3.38%, BaO 39.36%; The chemical composition of the diopside consists of the following components by weight: SiO2 56.49%, Al2O3 1.18%, Fe2O3 0.65%, CaO 23.24%, MgO 17.33%, K2O 0.06%, Na2O 0.41%, and LOI 0.64%.

4. The method for preparing the point-transmitting ceramic rock plate with relief effect according to claim 1 is characterized in that: The water-retaining zirconium-based ultra-white cosmetic soil described in step (2) is composed of the following components by weight: 30 to 40 parts of jade semi-emulsified body powder, 10 to 15 parts of ultrafine quartz powder, 10 to 20 parts of zircon white frit, 6 to 10 parts of calcined alumina powder, 1 to 3 parts of zirconium silicate, 10 to 15 parts of potassium feldspar, 5 to 8 parts of nepheline powder, 10 to 15 parts of ball clay, 2 to 3 parts of burnt talc, 0.5 to 1 part of sodium tripolyphosphate + sodium hexametaphosphate, 0 to 0.5 parts of sodium carboxymethyl cellulose, and 0.5 to 1.2 parts of water retaining agent.

5. The method for preparing the point-transmitting ceramic rock plate with relief effect according to claim 4 is characterized in that: The ultrafine quartz powder, calcined alumina powder and zirconium silicate are industrial-grade raw materials, and the introduced fineness is 325 mesh sieve, and the median particle size is 30±5μm; The potassium feldspar and nepheline powders have a fineness of 200 to 300 meshes; The zirconium white frit is a frit containing zirconium and having an initial melting temperature of 900-1000° C. The chemical composition of the zirconium white frit is composed of the following components by weight percentage: SiO2 61.24%, Al2O3 10.15%, Fe2O3 0.14%, CaO12.18%, MgO3.05%, K2O 4.07%, Na2O 1.15%, ZrO2 5.44%, ZnO 2.13%, LOI 0.45%; its introduction fineness is 150-250 mesh; The ball clay is a mixed clay mineral of montmorillonite, illite and kaolinite, and the chemical composition of the ball clay consists of the following components by weight percentage: SiO2 49.65%, Al2O3 34.92%, CaO 0.14%, MgO 0.33%, K2O 2.02%, Na2O0.10%, Fe2O3 1.51%, LOI 11.33%; The water retaining agent is a hydrophilic water retaining agent, the main component of which is a polyol, which is a composite solution of one or more of propylene glycol, glycerol, polyethylene glycol, and 1,3-butylene glycol.

6. The method for preparing the point-transmitting ceramic rock plate with relief effect according to claim 1, characterized in that: The bonding ink described in step (3) is composed of the following components by weight: 5 to 7 parts of zirconium oxide, 18 to 25 parts of a binder, 65 to 70 parts of an alcohol ether solvent, and 3 to 5 parts of a dispersant.

7. The method for preparing the point-transmitting ceramic rock plate with relief effect according to claim 6, characterized in that: The bonding ink is further composed of the following components by weight: 7 parts of zirconium oxide, 20 parts of a binder, 70 parts of an alcohol ether solvent, and 3 parts of a dispersant.

8. The method for preparing the point-transmitting ceramic rock plate with relief effect according to claim 1, characterized in that: The matte opacifying granular powder described in step (4) is composed of the following components by weight: 15 to 20 parts of barium-based frit, 10 to 20 parts of zirconium silicate, 30 to 50 parts of potassium feldspar powder, 10 to 15 parts of high-zinc low-temperature frit, 5 to 8 parts of strontium carbonate, 3 to 5 parts of kaolin, 0.5 to 1 part of sodium hexametaphosphate, and 0 to 0.3 part of sodium carboxymethyl cellulose.

9. The method for preparing the point-transmitting ceramic rock plate with relief effect according to claim 8, characterized in that: The high-zinc low-temperature frit has a ZnO weight percentage content of more than 10%, an initial melting temperature of 800-900°C, a high zinc content, and a low sintering temperature. The chemical composition of the high-zinc low-temperature frit is composed of the following components by weight percentage: SiO2 60.5%, Al2O3 9.1%, CaO 12.1%, MgO 2.2%, K2O 4.3%, Na2O 0.5%, and ZnO 11.3%.

10. The method for preparing the point-transmitting ceramic rock plate with relief effect according to claim 1 or 2, characterized in that: The jade semi-opaque body described in step (1) is further composed of the following components by weight: 17 parts of kaolin, 8 parts of black mud, 49 parts of glass frit, 4 parts of diopside, 6 parts of quartz powder, 11 parts of barium-based frit, 0.8 parts of organic additives, and 1 part of liquid dissolving agent; the chemical composition of the jade semi-opaque body is composed of the following components by weight percentage: SiO2 63.55%, Al2O3 17.65%, CaO 1.88%, MgO 2.23%, K2O 5.25%, Na2O 1.13%, Fe2O3 0.20%, BaO 4.32%, LOI 3.79%; the preparation method of the jade semi-emulsified body powder is as follows: the jade semi-emulsified body formula raw materials are subjected to graded ball milling, and after the ball milling reaches the qualified fineness, the mud is placed in the high-level pool for uniform stirring, and the mud control parameters are as follows: the fineness is 1.88% of the 325 mesh residue, the water content is 36.8%, the mud Engler viscosity is 83S, the D50 particle size is 7.79μm, and the spray drying and granulation are carried out using natural gas as the heat source to obtain the jade semi-emulsified body powder.

11. The method for preparing the point-transmitting ceramic rock plate with relief effect according to claim 1 or 4, characterized in that: The water-retaining zirconium-based ultra-white cosmetic soil described in step (2) is further composed of the following components by weight: 35 parts of jade semi-emulsified body powder, 12 parts of ultrafine quartz powder, 15 parts of zircon white frit, 6 parts of calcined alumina powder, 3 parts of zirconium silicate, 10 parts of potassium feldspar, 7 parts of nepheline powder, 10 parts of ball clay, 2 parts of burned talc, 0.7 parts of sodium tripolyphosphate + sodium hexamethaphosphate, 0.3 parts of sodium carboxymethyl cellulose, and 0.8 parts of water retaining agent; the chemical composition of the water-retaining zirconium-based ultra-white cosmetic soil is composed of the following components by weight percentage: SiO2 62.47%, Al2O3 22.95%, Fe2O3 0.15%, CaO 1.76%, MgO 2.13%, K2O 4.34%, Na2O1.68%, ZrO2 2.92%, BaO 1.60%; the preparation method of the water-retaining zirconium-based ultra-white cosmetic soil is as follows: according to the formula of the water-retaining zirconium-based ultra-white cosmetic soil, jade semi-emulsified green body powder, ultrafine quartz powder, zirconium white frit, calcined alumina powder, zirconium silicate, potassium feldspar, nepheline powder, ball clay, burned talc, sodium tripolyphosphate, sodium hexamethaphosphate, and sodium carboxymethyl cellulose are placed in a ball mill, and then 40 parts of water are added, and the ball mill is milled to a fineness of 0.4-0.7% after the residue on a 325-mesh sieve is removed, and after the removal of the slurry, a water-retaining agent is added to the slurry and stirred evenly, and then the slurry is deironed to control the iron content in the cosmetic soil slurry to be 0.13-0.15%.

12. The method for preparing the point-transmitting ceramic rock plate with relief effect according to claim 1 or 8, characterized in that: The matte opalescent granular powder described in step (4) is further composed of the following components by weight: 15 parts of barium-based frit, 20 parts of zirconium silicate, 40 parts of potassium feldspar powder, 15 parts of high-zinc low-temperature frit, 5 parts of strontium carbonate, 5 parts of kaolin, 0.78 parts of sodium hexametaphosphate, and 0.21 parts of sodium carboxymethyl cellulose. The chemical composition of the matte opalescent granular powder is composed of the following components by weight percentage: SiO2 56.68%, Al2O3 14.12%, CaO 1.91%, MgO 0.37%, K2O 4.82%, Na2O 1.33%, Fe2O3 0.12%, ZnO 1.73%, ZrO2 13.08%, SrO 3.60%, LOI 2.24%; the preparation method of the matte opalescent granular powder is as follows: weigh the matte opalescent granular powder according to the formula and put it into a ball mill, then add 40 parts of water, ball mill to a fineness of 0.15-0.35% of the residue on a 325-mesh sieve, and then adjust the glaze slurry to an Engler viscosity of 42S and a specific gravity of 1.82-1.91, and then use a spray dryer to make the slurry into powder particles, the moisture content of the powder particles is 1.8%, and the bulk density is 0.96g / cm 3 , and then put the obtained powder particles into a kiln for firing. The maximum firing temperature is controlled at 950-1020°C and the firing cycle is 6 hours to obtain a matte opacified granular powder product.

13. The method for preparing the point-transmitting ceramic rock plate with relief effect according to claim 1, characterized in that: The protective glaze described in step (7) is selected and adjusted according to the gloss and texture of the product development, and is preferably a matte spray protective glaze.

14. A ceramic rock plate with relief effect and point-transmitting light, characterized in that: The ceramic rock slab with relief effect and point-transmitting properties is prepared by the method for preparing the ceramic rock slab with relief effect and point-transmitting properties as described in any one of claims 1 to 9 and 13.

Citation Information

Patent Citations

  • Semi-transparency ceramic material, ceramic sheet and preparation method thereof

    CN101898891A

  • Light-transmitting ceramic tile with fixed-position crystal flowers and preparation method thereof

    CN110845227A

  • Ceramic rock plate with multicolor light-transmitting three-dimensional effect and manufacturing method thereof

    CN113896569A

  • Large crystal flower light transmitting jade brick

    CN109264993A

  • Formula and process of opaque porcelain

    CN114455942A