High-strength aluminum oxide ceramic and preparation method thereof
By using a combination of interfacial phase slurry and fiber carrier in alumina ceramic materials, combined with modified nanozirconia and plasticizer, the brittleness and defect sensitivity of alumina ceramic materials are solved, and its strength and toughness are significantly improved , improves the reliability and application potential of parts.
Patent Information
- Application Number
- CN202411121886.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
AI Technical Summary
The ionic covalent bonds of alumina ceramic materials hinder all ductile behaviors, resulting in their inherent brittleness and defect sensitivity, seriously affecting the service reliability of alumina ceramic materials parts and restricting their application in more fields.
Using the combination of interfacial phase slurry, fiber carrier, modified nanozirconia, plasticizer and crosslinking agent, the composite interfacial phase-encapsulated fiber carrier is prepared by ultrasonic stirring and ball milling, and sintered at high temperature. Treatment to improve the strength and fracture toughness of alumina ceramics.
It significantly improves the strength, fracture toughness and thermal shock resistance of alumina ceramics, reduces the sintering temperature, enhances the mechanical properties of the materials, and improves the reliability and application potential of the parts.
Smart Images

Figure CN118930233A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic materials, and in particular relates to a high-strength alumina ceramic and a preparation method thereof. Background Art
[0002] Ceramic materials have become an important part of modern new materials due to their excellent properties such as high strength, high temperature resistance, high hardness and corrosion resistance. Among them, alumina ceramics have extremely high application potential and value in various fields such as medicine, chemical industry, machinery, aerospace, etc. due to their excellent oxidation resistance, chemical stability and low cost.
[0003] Some invention patents in the field of ceramic material technology are disclosed in the prior art, among which the invention patent with application number CN201811069194.5 discloses a method for preparing alumina ceramics and the obtained products, which is characterized in that high-strength and uniformly structured alumina ceramics are prepared by gel injection molding process. Among them, the monomers of the injection system respectively use low-toxic N-hydroxymethyl acrylamide and α-methyl acrylic acid. In order to improve the high-temperature sintering performance of alumina powder, a high-temperature sintering aid is added. The compressive strength of the dried alumina ceramic green body is 15-20Mpa, and the density is 1.5-2.0g / cm3. The compressive strength of the alumina ceramic sintered at 1500℃ is 40-60MPa, and the density is 3.0-3.8g / cm3. Alumina ceramics prepared by gel injection molding have high density, high strength, and can achieve the purpose of near-net forming. The ionic covalent bonds of alumina ceramic materials hinder all ductile behaviors, resulting in their inherent brittleness and defect sensitivity, which seriously affects the service reliability of alumina ceramic parts and restricts their application in more fields.
[0004] Based on this, the present invention designs a high-strength alumina ceramic and a preparation method thereof to solve the above problems. Summary of the invention
[0005] The purpose of the present invention is to propose a high-strength alumina ceramic and a preparation method thereof in order to solve the problem that the ionic covalent bonds of alumina ceramic materials hinder all ductile behaviors, resulting in their inherent brittleness and defect sensitivity, seriously affecting the service reliability of alumina ceramic parts and restricting their application in more fields.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A high-strength alumina ceramic is prepared from the following raw materials in parts by weight: 80-100 parts of interface phase slurry, 20-30 parts of fiber carrier, 10-20 parts of modified nano zirconium oxide, 6-10 parts of plasticizer, 3-5 parts of crosslinking agent and 60-100 parts of water;
[0008] Preparation method of the interface phase slurry:
[0009] Add nano-aluminum oxide powder and hexagonal boron nitride powder into an ultrasonic stirring device at a volume ratio of 2:5 and mix them evenly;
[0010] After the nano-aluminum oxide powder and the hexagonal boron nitride powder are uniformly mixed, a dispersant and 2 wt% of a binder are sequentially added into the ultrasonic stirring device. At this time, the mass ratio of the interface phase powder to the binder in the ultrasonic stirring device is 18:1.
[0011] The mixed slurry in the ultrasonic stirring device is transferred to the planetary ball mill, and alumina grinding balls twice the mass of the powder are added to the planetary ball mill to improve the mixing uniformity;
[0012] After the planetary ball mill was operated for 26 hours, an interface phase slurry was obtained.
[0013] As a further description of the above technical solution:
[0014] The dispersant is deionized water, and the adhesive is polyethyleneimine.
[0015] As a further description of the above technical solution:
[0016] The preparation method of the fiber carrier:
[0017] Add the aluminum oxide chopped fibers into an ultrasonic cleaning device, remove the organic colloid and other impurities attached to the surface of the aluminum oxide chopped fibers, and then rinse them with distilled water for multiple times;
[0018] Add the interfacial phase slurry together with the rinsed aluminum oxide chopped fibers into an ultrasonic stirring device and continue ultrasonic stirring;
[0019] The ultrasonic stirring device is heated in a water bath, and after the excess water in the ultrasonic stirring device is completely evaporated, a fiber carrier wrapped by a composite interface phase is obtained.
[0020] As a further description of the above technical solution:
[0021] The plasticizer is any one or more combinations of polyethylene glycol, ethylene glycol, glycerol, paraffin and waterborne polyurethane, and the crosslinking agent is N,N-methylenebisacrylamide.
[0022] A method for preparing high-strength alumina ceramics comprises the following steps:
[0023] The fiber carrier wrapped with the composite interface phase is added into water to prepare a solution, and then modified nano zirconium oxide, a plasticizer, a cross-linking agent, yttrium-stabilized tetragonal zirconium oxide powder and a composite additive are added into the solution;
[0024] After being mixed evenly, the obtained slurry is ball-milled for 5-12 hours, and then vacuum-defoamed at 70-80°C for 20-50 minutes before injection molding with a filling pressure of 8-20MPa;
[0025] After curing and molding at room temperature, demould, dry to constant weight, put into a high-temperature furnace and heat to 520-600℃ for debinding for 1-2h, then heat to 1560-1610℃ for sintering for 2-4h, and cool to room temperature with the furnace.
[0026] As a further description of the above technical solution:
[0027] The preparation method of the modified nano zirconium oxide comprises the following steps:
[0028] The prepared fiber carrier wrapped with the composite interface phase is dissolved in hydrochloric acid and then mixed with an aqueous solution of zirconium oxychloride octahydrate to prepare a salt solution with a concentration of 1.0 mol%;
[0029] The salt solution is added in a mist state to the dilute ammonia water heated in a water bath, and is stirred rapidly during the addition of the salt solution to increase the nucleation rate during nucleation, so that the flocculation is small during precipitation and the precipitated particles are fine;
[0030] After the reaction between the salt solution and the dilute ammonia water is completed, the mixture is rinsed with anhydrous ethanol for multiple times to prevent agglomeration, and then dried and finely ground, sieved and calcined in sequence.
[0031] As a further description of the above technical solution:
[0032] The dilute ammonia water bath heating is stable and constant, the dilute ammonia water bath heating temperature is 42° C., and the pH value of the dilute ammonia water is 8.9.
[0033] As a further description of the above technical solution:
[0034] The sieving process is 800 mesh and the calcination temperature is 860°C.
[0035] As a further description of the above technical solution:
[0036] The addition of the yttrium-stabilized tetragonal zirconium oxide powder and the composite additive comprises the following steps:
[0037] 16 vol% yttrium-stabilized tetragonal zirconia powder was added to the alumina ceramic batch, followed by addition of composite additives in total amounts of 2.4% and 4.4% respectively;
[0038] After the addition of the composite additives is completed, a ball milling and mixing process is performed using a ball milling device for 10 hours, followed by a drying process. After screening, the mixture is first dry pressed and then statically pressed to obtain an alumina ceramic product body.
[0039] As a further description of the above technical solution:
[0040] The composite additive is any one or more combinations of magnesium oxide, silicate materials and rare earth compounds. The pressure environment of the dry pressing is 110 MPa, and the pressure environment of the static pressing is 190 MPa.
[0041] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0042] 1. In the present invention, short-cut aluminum oxide fibers are used as a matrix, and nano aluminum oxide powder and micron-sized hexagonal boron nitride powder are used as a composite interface phase to obtain a fiber carrier wrapped with a composite interface phase. Micron-sized hexagonal boron nitride is a two-dimensional layered structure material. The van der Waals force between layers is relatively weak, and micron-sized hexagonal boron nitride is prone to interlayer sliding under the action of shear force. In addition, due to its good chemical stability, the ceramic body based on aluminum oxide fibers is prevented from losing its toughening effect during the sintering process.
[0043] 2. In the present invention, the fiber carrier wrapped with the composite interface phase is wrapped with nano-alumina, thereby producing a good toughening effect during the phase change process. During the calcination process, its stress-strain state changes, which affects the martensitic phase transition temperature and the amount of phase transition nano-alumina precipitation under stress induction, thereby improving the strength, fracture toughness and thermal shock resistance of alumina ceramic products.
[0044] 3. In the present invention, composite additives are added and their comprehensive superposition effect is utilized. By adding a small amount of composite additives, not only the sintering temperature of alumina ceramics is significantly reduced, but also better mechanical properties are obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 A schematic diagram of a high-strength alumina ceramic and a preparation method thereof proposed in the present invention;
[0046] Figure 2 A schematic diagram of the process of preparing the interface phase slurry in a high-strength alumina ceramic and a preparation method thereof proposed by the present invention;
[0047] Figure 3 A schematic diagram of the process of preparing a fiber carrier in a high-strength alumina ceramic and a preparation method thereof proposed in the present invention;
[0048] Figure 4 A schematic diagram of the process of modifying nano zirconium oxide in a high-strength alumina ceramic and a preparation method thereof proposed by the present invention;
[0049] Figure 5The present invention provides a schematic diagram of the process of adding yttrium-stabilized tetragonal zirconia powder and composite additives in a high-strength alumina ceramic and a preparation method thereof. DETAILED DESCRIPTION
[0050] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] Embodiment 1
[0052] A high-strength alumina ceramic is prepared from the following raw materials in parts by weight: 80 parts of interface phase slurry, 20 parts of fiber carrier, 10 parts of modified nano zirconium oxide, 6 parts of plasticizer, 3-5 parts of crosslinking agent and 60 parts of water, wherein the dispersant is deionized water, the adhesive is polyethyleneimine, the plasticizer is any one or more combinations of polyethylene glycol, ethylene glycol, glycerol, paraffin and waterborne polyurethane, and the crosslinking agent is N,N-methylenebisacrylamide;
[0053] Preparation method of the interface phase slurry:
[0054] Add nano-aluminum oxide powder and hexagonal boron nitride powder into an ultrasonic stirring device at a volume ratio of 2:5 and mix them evenly;
[0055] After the nano-aluminum oxide powder and the hexagonal boron nitride powder are uniformly mixed, a dispersant and 2 wt% of a binder are sequentially added into the ultrasonic stirring device. At this time, the mass ratio of the interface phase powder to the binder in the ultrasonic stirring device is 18:1.
[0056] The mixed slurry in the ultrasonic stirring device is transferred to the planetary ball mill, and alumina grinding balls twice the mass of the powder are added to the planetary ball mill to improve the mixing uniformity;
[0057] After the planetary ball mill has been in operation for 26 hours, an interface phase slurry is obtained;
[0058] The preparation method of the fiber carrier:
[0059] Add the aluminum oxide chopped fibers into an ultrasonic cleaning device, remove the organic colloid and other impurities attached to the surface of the aluminum oxide chopped fibers, and then rinse them with distilled water for multiple times;
[0060] Add the interfacial phase slurry together with the rinsed aluminum oxide chopped fibers into an ultrasonic stirring device and continue ultrasonic stirring;
[0061] The ultrasonic stirring device is heated in a water bath, and after the excess water in the ultrasonic stirring device is completely evaporated, a fiber carrier wrapped by a composite interface phase is obtained;
[0062] A method for preparing high-strength alumina ceramics comprises the following steps:
[0063] The fiber carrier wrapped with the composite interface phase is added into water to prepare a solution, and then modified nano zirconium oxide, a plasticizer, a cross-linking agent, yttrium-stabilized tetragonal zirconium oxide powder and a composite additive are added into the solution;
[0064] After being mixed evenly, the obtained slurry was ball-milled for 5 h, and then vacuum-defoamed at 70 °C for 20 min before injection molding with a filling pressure of 8 MPa.
[0065] After curing at room temperature, demould, dry to constant weight, put into a high-temperature furnace and heat to 520℃ for debinding for 1h, then heat to 1560℃ for sintering for 2h, and cool to room temperature in the furnace;
[0066] The preparation method of the modified nano zirconium oxide comprises the following steps:
[0067] The prepared fiber carrier wrapped with the composite interface phase is dissolved in hydrochloric acid and then mixed with an aqueous solution of zirconium oxychloride octahydrate to prepare a salt solution with a concentration of 1.0 mol%;
[0068] The salt solution is added in a mist state to the dilute ammonia water heated in a water bath, and the salt solution is stirred rapidly during the process of adding the salt solution to increase the nucleation rate during nucleation, so that the flocculation is small during precipitation and the precipitated particles are fine. The dilute ammonia water bath is heated stably and constantly, the dilute ammonia water bath heating temperature is 42° C., and the pH value of the dilute ammonia water is 8.9;
[0069] After the reaction between the salt solution and the dilute ammonia solution is completed, the mixture is rinsed with anhydrous ethanol for multiple times to prevent agglomeration, and then dried and finely ground, sieved and calcined in sequence, wherein the sieve is 800 mesh and the calcination temperature is 860°C;
[0070] The addition of the yttrium-stabilized tetragonal zirconium oxide powder and the composite additive comprises the following steps:
[0071] 16 vol% yttrium-stabilized tetragonal zirconia powder was added to the alumina ceramic batch, followed by addition of composite additives in total amounts of 2.4% and 4.4% respectively;
[0072] After completing the addition of the composite additive, a ball milling and mixing treatment is performed for 10 hours using a ball mill, followed by a drying treatment. After screening treatment, dry pressing is performed first and then static pressing is performed to obtain an alumina ceramic product body. The composite additive is any one or more combinations of magnesium oxide, silicate substances and rare earth compounds. The dry pressing pressure environment is 110MPa, and the static pressing pressure environment is 190MPa.
[0073] Embodiment 2
[0074] A high-strength alumina ceramic is prepared from the following raw materials in parts by weight: 100 parts of interface phase slurry, 30 parts of fiber carrier, 20 parts of modified nano zirconium oxide, 10 parts of plasticizer, 5 parts of crosslinking agent and 100 parts of water, wherein the dispersant is deionized water, the adhesive is polyethyleneimine, the plasticizer is any one or more combinations of polyethylene glycol, ethylene glycol, glycerol, paraffin and waterborne polyurethane, and the crosslinking agent is N,N-methylenebisacrylamide;
[0075] Preparation method of the interface phase slurry:
[0076] Add nano-aluminum oxide powder and hexagonal boron nitride powder into an ultrasonic stirring device at a volume ratio of 2:5 and mix them evenly;
[0077] After the nano-aluminum oxide powder and the hexagonal boron nitride powder are uniformly mixed, a dispersant and 2 wt% of a binder are sequentially added into the ultrasonic stirring device. At this time, the mass ratio of the interface phase powder to the binder in the ultrasonic stirring device is 18:1.
[0078] The mixed slurry in the ultrasonic stirring device is transferred to the planetary ball mill, and alumina grinding balls twice the mass of the powder are added to the planetary ball mill to improve the mixing uniformity;
[0079] After the planetary ball mill has been in operation for 26 hours, an interface phase slurry is obtained;
[0080] The preparation method of the fiber carrier:
[0081] Add the aluminum oxide chopped fibers into an ultrasonic cleaning device, remove the organic colloid and other impurities attached to the surface of the aluminum oxide chopped fibers, and then rinse them with distilled water for multiple times;
[0082] Add the interfacial phase slurry together with the rinsed aluminum oxide chopped fibers into an ultrasonic stirring device and continue ultrasonic stirring;
[0083] The ultrasonic stirring device is heated in a water bath, and after the excess water in the ultrasonic stirring device is completely evaporated, a fiber carrier wrapped by a composite interface phase is obtained;
[0084] A method for preparing high-strength alumina ceramics comprises the following steps:
[0085] The fiber carrier wrapped with the composite interface phase is added into water to prepare a solution, and then modified nano zirconium oxide, a plasticizer, a cross-linking agent, yttrium-stabilized tetragonal zirconium oxide powder and a composite additive are added into the solution;
[0086] After being mixed evenly, the obtained slurry was ball-milled for 12 hours, and then vacuum-defoamed at 80°C for 50 minutes before injection molding with a filling pressure of 20 MPa.
[0087] After curing at room temperature, demould, dry to constant weight, put into a high-temperature furnace and heat to 600℃ for debinding for 2h, then heat to 1610℃ for sintering for 4h, and cool to room temperature in the furnace;
[0088] The preparation method of the modified nano zirconium oxide comprises the following steps:
[0089] The prepared fiber carrier wrapped with the composite interface phase is dissolved in hydrochloric acid and then mixed with an aqueous solution of zirconium oxychloride octahydrate to prepare a salt solution with a concentration of 1.0 mol%;
[0090] The salt solution is added in a mist state to the dilute ammonia water heated in a water bath, and the salt solution is stirred rapidly during the process of adding the salt solution to increase the nucleation rate during nucleation, so that the flocculation is small during precipitation and the precipitated particles are fine. The dilute ammonia water bath is heated stably and constantly, the dilute ammonia water bath heating temperature is 42° C., and the pH value of the dilute ammonia water is 8.9;
[0091] After the reaction between the salt solution and the dilute ammonia solution is completed, the mixture is rinsed with anhydrous ethanol for multiple times to prevent agglomeration, and then dried and finely ground, sieved and calcined in sequence, wherein the sieve is 800 mesh and the calcination temperature is 860°C;
[0092] The addition of the yttrium-stabilized tetragonal zirconium oxide powder and the composite additive comprises the following steps:
[0093] 16 vol% yttrium-stabilized tetragonal zirconia powder was added to the alumina ceramic batch, followed by addition of composite additives in total amounts of 2.4% and 4.4% respectively;
[0094] After completing the addition of the composite additive, a ball milling and mixing treatment is performed for 10 hours using a ball mill, followed by a drying treatment. After screening treatment, dry pressing is performed first and then static pressing is performed to obtain an alumina ceramic product body. The composite additive is any one or more combinations of magnesium oxide, silicate substances and rare earth compounds. The dry pressing pressure environment is 110MPa, and the static pressing pressure environment is 190MPa.
[0095] Embodiment 3
[0096] A high-strength alumina ceramic is prepared from the following raw materials in parts by weight: 90 parts of interface phase slurry, 25 parts of fiber carrier, 15 parts of modified nano zirconium oxide, 8 parts of plasticizer, 4 parts of cross-linking agent and 80 parts of water, wherein the dispersant is deionized water, the adhesive is polyethyleneimine, the plasticizer is any one or more combinations of polyethylene glycol, ethylene glycol, glycerol, paraffin and waterborne polyurethane, and the cross-linking agent is N,N-methylenebisacrylamide;
[0097] Preparation method of the interface phase slurry:
[0098] Add nano-aluminum oxide powder and hexagonal boron nitride powder into an ultrasonic stirring device at a volume ratio of 2:5 and mix them evenly;
[0099] After the nano-aluminum oxide powder and the hexagonal boron nitride powder are uniformly mixed, a dispersant and 2 wt% of a binder are sequentially added into the ultrasonic stirring device. At this time, the mass ratio of the interface phase powder to the binder in the ultrasonic stirring device is 18:1.
[0100] The mixed slurry in the ultrasonic stirring device is transferred to the planetary ball mill, and alumina grinding balls twice the mass of the powder are added to the planetary ball mill to improve the mixing uniformity;
[0101] After the planetary ball mill has been in operation for 26 hours, an interface phase slurry is obtained;
[0102] The preparation method of the fiber carrier:
[0103] Add the aluminum oxide chopped fibers into an ultrasonic cleaning device, remove the organic colloid and other impurities attached to the surface of the aluminum oxide chopped fibers, and then rinse them with distilled water for multiple times;
[0104] Add the interfacial phase slurry together with the rinsed aluminum oxide chopped fibers into an ultrasonic stirring device and continue ultrasonic stirring;
[0105] The ultrasonic stirring device is heated in a water bath, and after the excess water in the ultrasonic stirring device is completely evaporated, a fiber carrier wrapped by a composite interface phase is obtained;
[0106] A method for preparing high-strength alumina ceramics comprises the following steps:
[0107] The fiber carrier wrapped with the composite interface phase is added into water to prepare a solution, and then modified nano zirconium oxide, a plasticizer, a cross-linking agent, yttrium-stabilized tetragonal zirconium oxide powder and a composite additive are added into the solution;
[0108] After being mixed evenly, the obtained slurry was ball-milled for 8.5 h, and then vacuum-defoamed at 75 °C for 35 min before injection molding with a filling pressure of 14 MPa.
[0109] After curing at room temperature, demould, dry to constant weight, put into a high-temperature furnace and heat to 560℃ for debinding for 1.5h, then heat to 1585℃ for 3h, and cool to room temperature in the furnace;
[0110] The preparation method of the modified nano zirconium oxide comprises the following steps:
[0111] The prepared fiber carrier wrapped with the composite interface phase is dissolved in hydrochloric acid and then mixed with an aqueous solution of zirconium oxychloride octahydrate to prepare a salt solution with a concentration of 1.0 mol%;
[0112] The salt solution is added in a mist state to the dilute ammonia water heated in a water bath, and the salt solution is stirred rapidly during the process of adding the salt solution to increase the nucleation rate during nucleation, so that the flocculation is small during precipitation and the precipitated particles are fine. The dilute ammonia water bath is heated stably and constantly, the dilute ammonia water bath heating temperature is 42° C., and the pH value of the dilute ammonia water is 8.9;
[0113] After the reaction between the salt solution and the dilute ammonia solution is completed, the mixture is rinsed with anhydrous ethanol for multiple times to prevent agglomeration, and then dried and finely ground, sieved and calcined in sequence, wherein the sieve is 800 mesh and the calcination temperature is 860°C;
[0114] The addition of the yttrium-stabilized tetragonal zirconium oxide powder and the composite additive comprises the following steps:
[0115] 16 vol% yttrium-stabilized tetragonal zirconia powder was added to the alumina ceramic batch, followed by addition of composite additives in total amounts of 2.4% and 4.4% respectively;
[0116] After completing the addition of the composite additive, a ball milling and mixing treatment is performed for 10 hours using a ball mill, followed by a drying treatment. After screening treatment, dry pressing is performed first and then static pressing is performed to obtain an alumina ceramic product body. The composite additive is any one or more combinations of magnesium oxide, silicate substances and rare earth compounds. The dry pressing pressure environment is 110MPa, and the static pressing pressure environment is 190MPa.
[0117] Embodiment 4
[0118] A high-strength alumina ceramic is prepared from the following raw materials in parts by weight: 70 parts of interface phase slurry, 10 parts of fiber carrier, 5 parts of modified nano zirconium oxide, 4 parts of plasticizer, 2 parts of crosslinking agent and 40 parts of water, wherein the dispersant is deionized water, the adhesive is polyethyleneimine, the plasticizer is any one or more combinations of polyethylene glycol, ethylene glycol, glycerol, paraffin and waterborne polyurethane, and the crosslinking agent is N,N-methylenebisacrylamide;
[0119] Preparation method of the interface phase slurry:
[0120] Add nano-aluminum oxide powder and hexagonal boron nitride powder into an ultrasonic stirring device at a volume ratio of 2:5 and mix them evenly;
[0121] After the nano-aluminum oxide powder and the hexagonal boron nitride powder are uniformly mixed, a dispersant and 2 wt% of a binder are sequentially added into the ultrasonic stirring device. At this time, the mass ratio of the interface phase powder to the binder in the ultrasonic stirring device is 18:1.
[0122] The mixed slurry in the ultrasonic stirring device is transferred to the planetary ball mill, and alumina grinding balls twice the mass of the powder are added to the planetary ball mill to improve the mixing uniformity;
[0123] After the planetary ball mill has been in operation for 26 hours, an interface phase slurry is obtained;
[0124] The preparation method of the fiber carrier:
[0125] Add the aluminum oxide chopped fibers into an ultrasonic cleaning device, remove the organic colloid and other impurities attached to the surface of the aluminum oxide chopped fibers, and then rinse them with distilled water for multiple times;
[0126] Add the interfacial phase slurry together with the rinsed aluminum oxide chopped fibers into an ultrasonic stirring device and continue ultrasonic stirring;
[0127] The ultrasonic stirring device is heated in a water bath, and after the excess water in the ultrasonic stirring device is completely evaporated, a fiber carrier wrapped by a composite interface phase is obtained;
[0128] A method for preparing high-strength alumina ceramics comprises the following steps:
[0129] The fiber carrier wrapped with the composite interface phase is added into water to prepare a solution, and then modified nano zirconium oxide, a plasticizer, a cross-linking agent, yttrium-stabilized tetragonal zirconium oxide powder and a composite additive are added into the solution;
[0130] After being mixed evenly, the obtained slurry was ball-milled for 4 h, and then vacuum-defoamed at 60 °C for 10 min before injection molding with a filling pressure of 4 MPa.
[0131] After curing at room temperature, demould, dry to constant weight, put into a high-temperature furnace and heat to 500℃ for debinding for 0.6h, then heat to 1500℃ for 1h, and cool to room temperature in the furnace;
[0132] The preparation method of the modified nano zirconium oxide comprises the following steps:
[0133] The prepared fiber carrier wrapped with the composite interface phase is dissolved in hydrochloric acid and then mixed with an aqueous solution of zirconium oxychloride octahydrate to prepare a salt solution with a concentration of 1.0 mol%;
[0134] The salt solution is added in a mist state to the dilute ammonia water heated in a water bath, and the salt solution is stirred rapidly during the process of adding the salt solution to increase the nucleation rate during nucleation, so that the flocculation is small during precipitation and the precipitated particles are fine. The dilute ammonia water bath is heated stably and constantly, the dilute ammonia water bath heating temperature is 42° C., and the pH value of the dilute ammonia water is 8.9;
[0135] After the reaction between the salt solution and the dilute ammonia solution is completed, the mixture is rinsed with anhydrous ethanol for multiple times to prevent agglomeration, and then dried and finely ground, sieved and calcined in sequence, wherein the sieve is 800 mesh and the calcination temperature is 860°C;
[0136] The addition of the yttrium-stabilized tetragonal zirconium oxide powder and the composite additive comprises the following steps:
[0137] 16 vol% yttrium-stabilized tetragonal zirconia powder was added to the alumina ceramic batch, followed by addition of composite additives in total amounts of 2.4% and 4.4% respectively;
[0138] After completing the addition of the composite additive, a ball milling and mixing treatment is performed for 10 hours using a ball mill, followed by a drying treatment. After screening treatment, dry pressing is performed first and then static pressing is performed to obtain an alumina ceramic product body. The composite additive is any one or more combinations of magnesium oxide, silicate substances and rare earth compounds. The dry pressing pressure environment is 110MPa, and the static pressing pressure environment is 190MPa.
[0139] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A high-strength alumina ceramic, characterized in that: The invention is prepared from the following raw materials in parts by weight: 80-100 parts of interface phase slurry, 20-30 parts of fiber carrier, 10-20 parts of modified nano zirconium oxide, 6-10 parts of plasticizer, 3-5 parts of crosslinking agent and 60-100 parts of water; Preparation method of the interface phase slurry: Add nano-aluminum oxide powder and hexagonal boron nitride powder into an ultrasonic stirring device at a volume ratio of 2:5 and mix them evenly; After the nano-aluminum oxide powder and the hexagonal boron nitride powder are uniformly mixed, a dispersant and 2 wt% of a binder are sequentially added into the ultrasonic stirring device. At this time, the mass ratio of the interface phase powder to the binder in the ultrasonic stirring device is 18:
1. The mixed slurry in the ultrasonic stirring device is transferred to the planetary ball mill, and alumina grinding balls twice the mass of the powder are added to the planetary ball mill to improve the mixing uniformity; After the planetary ball mill was operated for 26 hours, an interface phase slurry was obtained.
2. A high-strength alumina ceramic according to claim 1, characterized in that: The dispersant is deionized water, and the adhesive is polyethyleneimine.
3. The high-strength alumina ceramic according to claim 1, characterized in that: The preparation method of the fiber carrier: Add the aluminum oxide chopped fibers into an ultrasonic cleaning device, remove the organic colloid and other impurities attached to the surface of the aluminum oxide chopped fibers, and then rinse them with distilled water for multiple times; Add the interfacial phase slurry together with the rinsed aluminum oxide chopped fibers into an ultrasonic stirring device and continue ultrasonic stirring; The ultrasonic stirring device is heated in a water bath, and after the excess water in the ultrasonic stirring device is completely evaporated, a fiber carrier wrapped by a composite interface phase is obtained.
4. The high-strength alumina ceramic according to claim 1, characterized in that: The plasticizer is any one or more combinations of polyethylene glycol, ethylene glycol, glycerol, paraffin and waterborne polyurethane, and the crosslinking agent is N,N-methylenebisacrylamide.
5. A method for preparing high-strength alumina ceramics according to any one of claim 1, characterized in that: The following steps are involved: The fiber carrier wrapped with the composite interface phase is added into water to prepare a solution, and then modified nano zirconium oxide, a plasticizer, a cross-linking agent, yttrium-stabilized tetragonal zirconium oxide powder and a composite additive are added into the solution; After mixing evenly, the obtained slurry is ball-milled for 5-12 hours, and then vacuum-defoamed at 70-80°C for 20-50 minutes before injection molding with a filling pressure of 8-20MPa; After curing and molding at room temperature, demould, dry to constant weight, put into a high-temperature furnace and heat to 520-600℃ for debinding for 1-2h, then heat to 1560-1610℃ for sintering for 2-4h, and cool to room temperature with the furnace.
6. The method for preparing a high-strength alumina ceramic according to claim 5, characterized in that: The preparation method of the modified nano zirconium oxide comprises the following steps: The prepared fiber carrier wrapped with the composite interface phase is dissolved in hydrochloric acid and then mixed with an aqueous solution of zirconium oxychloride octahydrate to prepare a salt solution with a concentration of 1.0 mol%; The salt solution is added in a mist state to the dilute ammonia water heated in a water bath, and is stirred rapidly during the addition of the salt solution to increase the nucleation rate during nucleation, so that the flocculation is small during precipitation and the precipitated particles are fine; After the reaction between the salt solution and the dilute ammonia water is completed, the mixture is rinsed with anhydrous ethanol for multiple times to prevent agglomeration, and then dried and finely ground, sieved and calcined in sequence.
7. The method for preparing a high-strength alumina ceramic according to claim 6, characterized in that: The dilute ammonia water bath heating is stable and constant, the dilute ammonia water bath heating temperature is 42° C., and the pH value of the dilute ammonia water is 8.
9.
8. The method for preparing a high-strength alumina ceramic according to claim 6, characterized in that: The sieving process is 800 mesh and the calcination temperature is 860°C.
9. The method for preparing a high-strength alumina ceramic according to claim 5, characterized in that: The addition of the yttrium-stabilized tetragonal zirconium oxide powder and the composite additive comprises the following steps: 16 vol% yttrium-stabilized tetragonal zirconia powder was added to the alumina ceramic batch, followed by addition of composite additives in total amounts of 2.4% and 4.4% respectively; After the addition of the composite additives is completed, a ball milling and mixing process is performed using a ball milling device for 10 hours, followed by a drying process. After screening, the mixture is first dry pressed and then statically pressed to obtain an alumina ceramic product body.
10. The method for preparing a high-strength alumina ceramic according to claim 9, characterized in that: The composite additive is any one or more combinations of magnesium oxide, silicate materials and rare earth compounds. The pressure environment of the dry pressing is 110 MPa, and the pressure environment of the static pressing is 190 MPa.
Citation Information
Patent Citations
Synergistic toughening alumina ceramic and preparation method thereof
CN101948325A
Zirconia / alumina ceramic composite material and preparation method thereof
CN113416064A
Method for modifying nano zirconium oxide powder by wet process
CN113800906A
High-damage-tolerance aluminum oxide composite ceramic and preparation method thereof
CN116102342A