Aluminum-silicon-calcium multiphase material and preparation method thereof

By adding TiO2 micropowder to the mixed material of bauxite and limestone, the sintering activity of the aluminum-silicon calcium composite material is improved, and the problems of low sintering activity and volume expansion effects are solved, and the dense material is obtained at a lower temperature is achieved, thus reducing the reduction of Production energy consumption and improve production efficiency.

CN118930240APending Publication Date: 2024-11-12SHANXI INST OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411158087.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the process of preparing aluminum-silicon calcium composite materials in solid phase synthesis, the reaction between the components leads to a volume expansion effect to inhibit the sintering process. Moreover, the sintering activity of mullite phase, calcium feldspar phase and corundum phase is low, which is difficult to Sintering at lower temperatures results in dense material.

Method used

Add TiO2 micro powder as a sintering agent to the mixture of bauxite and limestone. Through the sintering process, TiO2 is dissolved into the mullite phase, calcium feldspar phase, and corundum phase, thereby improving its sintering activity and promoting its growth, realizing the Sintering at lower temperatures and short time.

Benefits of technology

It significantly improves the sintering activity of mullite phase, calcium feldspar phase and corundum phase, and can obtain dense aluminum-silicon calcium composite materials at a lower sintering temperature and short time, reducing production energy consumption and improving production efficiency, and promoting The industry has achieved energy conservation, emission reduction and sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930240A_ABST
    Figure CN118930240A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of inorganic non-metallic materials, and particularly relates to an aluminum-silicon-calcium multiphase material and a preparation method thereof. The aluminum-silicon-calcium multiphase material disclosed by the invention is prepared from the following chemical components in percentage by mass: 36.7%-78.8% of Al2O3, 14.3%-42.7% of SiO2, 0.2%-20.6% of CaO and 1.0%-3.0% of TiO2, and the sum of the mass percentages of all the chemical components is 100%. The preparation method of the aluminum-silicon-calcium multiphase material comprises the following steps: crushing bauxite, limestone and TiO2, and mixing to obtain a mixed material; and pressing the mixed material into a green body, and sintering to obtain the aluminum-silicon-calcium multiphase material. The sintering activity of the mullite phase, the anorthite phase and the corundum phase is improved, the compact aluminum-silicon-calcium multiphase material can be obtained at a low sintering temperature for a short sintering time, the production energy consumption can be effectively reduced, and the production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inorganic non-metallic materials, and specifically relates to an aluminum-silicon-calcium composite material and a preparation method thereof. Background Art

[0002] Bauxite resources are abundant worldwide, providing excellent natural conditions for economic development. Bauxite is a natural raw material for electrolytic aluminum and refractory industries, and is widely used in the field of refractory materials. However, affected by the problem of bauxite resources worldwide, its price continues to rise, resulting in an increase in the production cost of aluminum refractory materials year by year. In particular, the rapid development of alumina production, excessive mining and production and processing have led to a rapid decline in the reserves of bauxite resources in my country, and resources are becoming increasingly scarce. The contradiction in the supply of high-grade bauxite is particularly prominent. Therefore, in order to ensure the long-term development of the aluminum industry and the refractory industry, it is necessary to strengthen research on improving the quality and efficiency of bauxite resources.

[0003] Mullite in Al2O3-SiO2 material, namely A3S2, has a melting point of 1840℃. It is widely used as refractory material in metallurgy, ceramics, glass, casting and other industries due to its high temperature resistance, high strength, low thermal conductivity, significant energy saving effect, good thermal stability and corrosion resistance.

[0004] Calcium feldspar in Al2O3-SiO2-CaO materials, namely CAS2, has a melting point of 1553℃. Due to its low thermal conductivity, low thermal expansion coefficient, small volume density, high specific strength, and small dielectric constant, it exhibits good thermal insulation effect and has the characteristics of high temperature resistance and corrosion resistance. Therefore, calcium feldspar has broad application prospects in the fields of metallurgy, chemistry, ceramics, and electronic equipment. Figure 1 As shown in the figure, when the Al2O3-SiO2-CaO ternary phase diagram is located in the lower right corner of mullite, i.e. A3S2, with a melting point of 1890°C, calcium feldspar, i.e. CAS2, with a melting point of 1553°C, and corundum, i.e. Al2O3, with a melting point of 2050°C, and the three connecting lines are in the Al2O3-A3S2-CAS2 sub-triangle area, the lowest eutectic temperature is ≥1512°C. Theoretically, by controlling the composition of Al2O3, SiO2, and CaO raw materials, it is entirely possible to prepare Al2O3-SiO2-CaO system composite materials with a crystal phase composition of mullite, calcium feldspar, and corundum or a combination of two of them. These materials have broad application prospects in the field of high-temperature industrial refractory materials for metallurgy, cement, glass, ceramics, petrochemicals, and electronic equipment.

[0005] As we all know, preparing composite materials from two or more materials with different properties can achieve complementary advantages and synergistic effects in performance, so that the overall performance of the composite material exceeds that of its base material. Given that bauxite resources worldwide generally contain two main components, Al2O3 and SiO2, this provides a natural advantage for using low-, medium- and high-grade natural bauxite, supplemented by a wide range of low-cost limestone raw materials worldwide, to manufacture aluminum-silicon-calcium composite materials through proportioning, while effectively broadening the range of raw material selection and providing technical possibilities for reducing the production cost of materials.

[0006] However, in the process of solid phase synthesis to prepare aluminum-silicon-calcium composite materials, the volume expansion effect associated with the reaction between the components inhibits the sintering process. At the same time, due to the low sintering activity of mullite phase, calcium feldspar phase and corundum phase, it is difficult to sinter at a lower temperature to obtain aluminum-silicon-calcium composite materials. Summary of the invention

[0007] In view of the problems existing in the prior art, the present invention provides an aluminum-silicon-calcium composite material and a preparation method thereof, wherein the aluminum-silicon-calcium composite material is prepared by adding TiO2 micropowder to a mixture of bauxite and limestone and then sintering. The sintering activity of the mullite phase, the anorthite phase, and the corundum phase is not only significantly improved, but also the growth of the mullite phase, the anorthite phase, and the corundum phase is further promoted, and a dense aluminum-silicon-calcium composite material can be obtained at a lower sintering temperature and a shorter insulation time, while also effectively reducing production energy consumption and improving production efficiency, which is of great significance for promoting energy conservation, emission reduction, and sustainable development in the industry.

[0008] To achieve the above object, the present invention adopts the following technical solutions:

[0009] The first object of the present invention is to provide an aluminum-silicon-calcium composite material, which is composed of the following raw materials in mass percentage: Al2O3 36.7% to 78.8%, SiO2 14.3% to 42.7%, CaO 0.2% to 20.6% and TiO2 1.0% to 3.0%, and the sum of the mass percentages of each raw material is 100%.

[0010] Preferably, the aluminum-silicon-calcium composite material is composed of the following raw materials in percentage by mass: Al2O3 39.8% to 76.7%, SiO2 15.6% to 39.6%, CaO 1.0% to 18.6% and TiO2 2.0% to 3.0%.

[0011] Preferably, the relative density of the aluminum-silicon-calcium composite material is 90.1% to 92.7%, wherein the relative density is measured according to the Archimedean principle.

[0012] Preferably, the apparent porosity of the aluminum-silicon-calcium composite material is 3.2% to 4.9%, wherein the apparent porosity is measured according to the Archimedean principle.

[0013] The second object of the present invention is to provide a method for preparing an aluminum-silicon-calcium composite material, which is prepared according to the following steps:

[0014] S1, using bauxite and limestone as raw materials, crushing the bauxite and the limestone and mixing them to obtain a first mixed material;

[0015] S2, using TiO2 as a sintering aid, mixing the sintering aid with the first mixed material and then pressing to obtain a green body;

[0016] S3. Sintering the green body at a heating rate of 5°C / min to 10°C / min to obtain an aluminum-silicon-calcium composite material.

[0017] Preferably, in step S1, in the first mixed material, the particle size of bauxite and limestone is ≤88 mesh; wherein, when the particle size is too large, the sintering time is prolonged and the sintering rate is reduced.

[0018] Preferably, in step S1, the mass of the bauxite accounts for 75% to 99% of the first mixed material.

[0019] Preferably, the purity of the TiO2 is ≥98.0% and the particle size is ≤10 μm; wherein, if the particle size of the TiO2 is greater than 10 μm, the amount of TiO2 used must be increased in order to obtain an aluminum-silicon-calcium composite material with the same volume density and porosity.

[0020] Preferably, in step S2, when pressing into a green body, the pressure applied is 110 MPa to 150 MPa.

[0021] Preferably, the mass ratio of TiO2 to the first mixed material is 1 to 3:100.

[0022] Preferably, in step S3, the sintering temperature is 1400° C. to 1500° C., and the sintering time is 2 h to 3 h.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The present invention provides an aluminum-silicon-calcium composite material, which is sintered by adding TiO2 powder to a mixture of bauxite and limestone, thereby not only significantly improving the sintering activity of mullite phase, anorthite phase and corundum phase, but also further promoting the growth of mullite phase, anorthite phase and corundum phase, and being able to obtain a dense aluminum-silicon-calcium composite material under conditions of lower sintering temperature and shorter insulation time, while effectively reducing production energy consumption and improving production efficiency, which is of great significance for promoting energy conservation, emission reduction and sustainable development in the industry.

[0025] 2. The present invention provides a method for preparing an aluminum-silicon-calcium composite material, comprising crushing bauxite and limestone to a particle size of ≤88 mesh to ensure the fineness and uniformity of the raw materials; then, mixing the mixture in a sand mixer to obtain a first mixed material; adding TiO2 powder to the first mixed material for mixing to obtain a second mixed material; pressing the second mixed material into a green body through a ball press; and sintering the green body to obtain an aluminum-silicon-calcium composite material.

[0026] Among them, during the sintering process, TiO2 micropowder is dissolved into the mullite phase, calcium feldspar phase and corundum phase, causing lattice distortion of the mullite phase, calcium feldspar phase and corundum phase, improving their activity, and promoting their sintering and densification behavior, so that aluminum-silicon-calcium composite materials can be obtained under lower secondary sintering temperature and shorter insulation time conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is the ternary phase diagram of Al2O3-SiO2-CaO system;

[0028] Figure 2 This is a flow chart for preparing the aluminum-silicon-calcium composite material of the present invention;

[0029] Figure 3 This is the XRD diagram of the aluminum-silicon-calcium composite material of Example 1 of the present invention;

[0030] Figure 4 This is a microstructure photograph of the aluminum-silicon-calcium composite material of Example 1 of the present invention;

[0031] Figure 5 This is a microstructure photograph of the aluminum-silicon-calcium composite material of Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The technical solution of the present invention will be clearly and completely described below in combination with the data in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] It should be noted that the professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods. The equipment used for mixing materials in the embodiments of the present invention is a S1110 sand mixer, the equipment used for pressing into balls is a GY650-180 ball press, the equipment used for sintering is a high-temperature vertical kiln, and the bauxite, limestone and TiO2 powder used are commercially available products; the mass fraction of Al2O3 in the bauxite used in the embodiments of the present invention is ≥42.0%, and the mass fraction of the effective component CaO in the limestone is ≥50.2%.

[0034] Compared with the prior art, the present invention overcomes the technical defect that the volume expansion effect accompanied by the reaction between the components inhibits the sintering process during the solid phase synthesis process of preparing aluminum-silicon-calcium composite materials by adding TiO2 micropowder as a sintering aid to the mixture of bauxite and limestone. At the same time, the present invention significantly improves the sintering activity of the mullite phase, calcium feldspar phase, and corundum phase by dissolving the TiO2 micropowder into the mullite phase, calcium feldspar phase, and corundum phase to form a solid solution during the sintering process, and promotes their sintering and densification behavior, thereby overcoming the technical problem that it is difficult to sinter the aluminum-silicon-calcium composite material at a relatively low temperature due to the low sintering activity of the mullite phase, calcium feldspar phase, and corundum phase.

[0035] On the one hand, the present invention provides an aluminum-silicon-calcium composite material, which is composed of the following raw materials in mass percentage: Al2O3 36.7%~78.8%, SiO2 14.3%~42.7%, CaO 0.2%~20.6% and TiO2 1.0%~3.0%, and the sum of the mass percentages of each raw material is 100%.

[0036] On the other hand, the present invention provides a method for preparing an aluminum-silicon-calcium composite material, comprising the following steps: crushing bauxite and limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material; adding TiO2 to the first mixed material and mixing them to obtain a second mixed material; pressing the second mixed material into a green body by a ball press at a pressure of 110MPa to 150MPa; and sintering the green body at 1400°C to 1500°C for 2h to 3h to obtain an aluminum-silicon-calcium composite material. The preparation process is as follows: Figure 2 shown.

[0037] In the present invention, the pressure of the aluminum-silicon-calcium composite material when pressed into a green body is any specific value between 110MPa and 150PMPa, such as 150MPa, 140MPa, 130MPa, 120MPa, and 110MPa; the sintering temperature is any specific value between 1400°C and 1500°C, such as 1500°C, 1450°C, and 1400°C; the sintering time is any specific value between 2h and 3h, such as 3h, 2.5h, and 2h. However, it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable, so they will not be repeated here.

[0038] The technical solution of the present invention is further explained by using embodiments below, which are specifically as follows:

[0039] Example 1

[0040] A method for preparing an aluminum-silicon-calcium composite material comprises the following steps:

[0041] S1, weighing 98.0% bauxite and 2.0% limestone, which account for 98.0% of the weight of the mixed material, crushing the bauxite and the limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material;

[0042] S2, weighing TiO2 at a weight ratio of 3.0% of the mixed material, adding it to the first mixed material for mixing, to obtain a second mixed material;

[0043] S3, pressing the second mixed material into a green compact by a ball press at a pressure of 150 MPa;

[0044] S4, keeping the green body at 1500° C. for 3 h and sintering it to obtain an aluminum-silicon-calcium composite material;

[0045] The mass percentage of each component of the aluminum-silicon-calcium composite material is Al2O3:SiO2:CaO:TiO2=61.9%:34.1%:1.0%:3.0%; the relative density is 90.6% and the apparent porosity is 4.8%.

[0046] Example 2

[0047] A method for preparing an aluminum-silicon-calcium composite material comprises the following steps:

[0048] S1, weighing 90.7% of bauxite and 9.3% of limestone in weight ratio of the mixed material, crushing the bauxite and limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material;

[0049] S2, weighing TiO2 at a weight ratio of 2.8% of the mixed material, adding it to the first mixed material for mixing, to obtain a second mixed material;

[0050] S3, pressing the second mixed material into a green compact by a ball press at a pressure of 140 MPa;

[0051] S4, keeping the green body at 1500° C. for 3 hours and sintering it to obtain an aluminum-silicon-calcium composite material;

[0052] The mass percentages of the components of the aluminum-silicon-calcium composite material are Al2O3:SiO2:CaO:TiO2=76.7%:15.6%:4.9%:2.8%; the relative density is 91.2% and the apparent porosity is 4.3%.

[0053] Example 3

[0054] A method for preparing an aluminum-silicon-calcium composite material comprises the following steps:

[0055] S1, weighing 85.3% of bauxite and 14.7% of limestone in weight ratio of the mixed material, crushing the bauxite and limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material;

[0056] S2, weighing TiO2 at a weight ratio of 2.1% of the mixed material, adding it to the first mixed material and mixing them to obtain a second mixed material;

[0057] S3, pressing the second mixed material into a green compact at a pressure of 130 MPa using a pellet press;

[0058] S4, keeping the green body at 1450° C. for 2.5 hours and sintering it to obtain an aluminum-silicon-calcium composite material;

[0059] The mass percentages of the components of the aluminum-silicon-calcium composite material are Al2O3:SiO2:CaO:TiO2=66.8%:23.7%:7.4%:2.1%; the relative density is 91.8% and the apparent porosity is 3.9%.

[0060] Example 4

[0061] A method for preparing an aluminum-silicon-calcium composite material comprises the following steps:

[0062] S1, weighing 82.9% of bauxite and 17.1% of limestone in weight ratio of the mixed material, crushing the bauxite and limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material;

[0063] S2, weighing TiO2 at a weight ratio of 2.5% of the mixed material, adding it to the first mixed material and mixing them to obtain a second mixed material;

[0064] S3, pressing the second mixed material into a green compact by a ball press at a pressure of 120 MPa;

[0065] S4, keeping the green body at 1450° C. for 2 h and sintering it to obtain an aluminum-silicon-calcium composite material;

[0066] The mass percentages of the components of the aluminum-silicon-calcium composite material are Al2O3:SiO2:CaO:TiO2=63.7%:19.9%:13.9%:2.5%; the relative density is 92.2% and the apparent porosity is 3.6%.

[0067] Example 5

[0068] A method for preparing an aluminum-silicon-calcium composite material comprises the following steps:

[0069] S1, weighing 80.0% bauxite and 20.0% limestone in weight ratio of the mixed material, crushing the bauxite and limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material;

[0070] S2, weighing TiO2 at a weight ratio of 2.0% of the mixed material, adding it to the first mixed material and mixing them to obtain a second mixed material;

[0071] S3, pressing the second mixed material into a green compact by a ball press at a pressure of 110 MPa;

[0072] S4, keeping the green body at 1400° C. for 2 h and sintering it to obtain an aluminum-silicon-calcium composite material;

[0073] The mass percentages of the components of the aluminum-silicon-calcium composite material are Al2O3:SiO2:CaO:TiO2=39.8%:39.6%:18.6%:2.0%; the relative density is 92.7% and the apparent porosity is 3.2%.

[0074] Example 6

[0075] A method for preparing an aluminum-silicon-calcium composite material comprises the following steps:

[0076] S1, weighing 99.0% bauxite and 1.0% limestone, which account for 99.0% of the weight of the mixed material, crushing the bauxite and the limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material;

[0077] S2, weighing TiO2 at a weight ratio of 3.0% of the mixed material, adding it to the first mixed material and mixing them to obtain a second mixed material;

[0078] S3, pressing the second mixed material into a green compact by a ball press at a pressure of 150 MPa;

[0079] S4, keeping the green body at 1500° C. for 3 hours and sintering it to obtain an aluminum-silicon-calcium composite material;

[0080] The mass percentage of each component of the aluminum-silicon-calcium composite material is Al2O3:SiO2:CaO:TiO2=78.8%:17.7%:0.5%:3.0%; the relative density is 90.5% and the apparent porosity is 4.6%.

[0081] Example 7

[0082] A method for preparing an aluminum-silicon-calcium composite material comprises the following steps:

[0083] S1, weighing 75.0% of bauxite and 25.0% of limestone in weight ratio of the mixed material, crushing the bauxite and limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material;

[0084] S2, weighing TiO2 at a weight ratio of 1.0% of the mixed material, adding it to the first mixed material and mixing them to obtain a second mixed material;

[0085] S3, pressing the second mixed material into a green compact by a ball press at a pressure of 110 MPa;

[0086] S4, keeping the green body at 1400° C. for 2 h and sintering it to obtain an aluminum-silicon-calcium composite material;

[0087] The mass percentages of the components of the aluminum-silicon-calcium composite material are Al2O3:SiO2:CaO:TiO2=36.7%:41.7%:20.6%:1.0%; the relative density is 90.1% and the apparent porosity is 4.9%.

[0088] Example 8

[0089] A method for preparing an aluminum-silicon-calcium composite material comprises the following steps:

[0090] S1, weighing 85.2% of bauxite and 14.8% of limestone in weight ratio of the mixed material, crushing the bauxite and limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material;

[0091] S2, weighing TiO2 at a weight ratio of 2.0% of the mixed material, adding it to the first mixed material and mixing them to obtain a second mixed material;

[0092] S3, pressing the second mixed material into a green compact by a ball press at a pressure of 120 MPa;

[0093] S4, keeping the green body at 1450° C. for 2 h and sintering it to obtain an aluminum-silicon-calcium composite material;

[0094] The mass percentages of the components of the aluminum-silicon-calcium composite material are Al2O3:SiO2:CaO:TiO2=47.8%:42.7%:7.5%:2.0%; the relative density is 90.3% and the apparent porosity is 4.7%.

[0095] Comparative Example 1

[0096] A method for preparing an aluminum-silicon-calcium composite material comprises the following steps:

[0097] S1, weighing 76.5% of bauxite and 23.5% of limestone in weight ratio of the mixed material, crushing the bauxite and limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material;

[0098] S2, pressing the mixed material into a green body at a pressure of 110 MPa through a ball press;

[0099] S3, keeping the green body at 1400° C. for 3 h and sintering it to obtain an aluminum-silicon-calcium composite material;

[0100] The mass percentages of the components of the aluminum-silicon-calcium composite material are Al2O3:SiO2:CaO=52.6%:32.8%:14.6%; the relative density is 52.2% and the apparent porosity is 40.3%.

[0101] Comparative Example 2

[0102] A method for preparing an aluminum-silicon-calcium composite material comprises the following steps:

[0103] S1, weighing 73.7% of bauxite and 26.3% of limestone in weight ratio of the mixed material, crushing the bauxite and limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material;

[0104] S2, pressing the mixed material into a green body at a pressure of 120 MPa through a ball press;

[0105] S3, keeping the green body at 1500° C. for 2.5 hours and sintering it to obtain an aluminum-silicon-calcium composite material;

[0106] The mass percentage of each component of the aluminum-silicon-calcium composite material is Al2O3:SiO2:CaO=48.6%:34.9%:16.5%; the relative density is 45.1% and the apparent porosity is 48.3%.

[0107] Comparative Example 3

[0108] A method for preparing an aluminum-silicon-calcium composite material comprises the following steps:

[0109] S1, weighing 70.7% of bauxite and 29.3% of limestone, crushing the bauxite and limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material;

[0110] S2, pressing the mixed material into a green body at a pressure of 130 MPa through a ball press;

[0111] S3, keeping the green body at 1450° C. for 2.5 hours and sintering it to obtain an aluminum-silicon-calcium composite material;

[0112] The mass percentages of the components of the aluminum-silicon-calcium composite material are Al2O3:SiO2:CaO=41.9%:39.6%:18.5%; the relative density is 37.3% and the apparent porosity is 57.3%.

[0113] Comparative Example 4

[0114] A method for preparing an aluminum-silicon-calcium composite material comprises the following steps:

[0115] S1, weighing 68.6% of bauxite and 31.4% of limestone, crushing the bauxite and limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material;

[0116] S2, pressing the mixed material into a green body at a pressure of 140 MPa through a ball press;

[0117] S3, keeping the green body at 1450° C. for 2 h and sintering it to obtain an aluminum-silicon-calcium composite material;

[0118] The mass percentages of the components of the aluminum-silicon-calcium composite material are Al2O3:SiO2:CaO=38.0%:42.1%:19.9%; the relative density is 29.7% and the apparent porosity is 65.6%.

[0119] Comparative Example 5

[0120] A method for preparing an aluminum-silicon-calcium composite material comprises the following steps:

[0121] S1, weighing 68.4% of bauxite and 31.6% of limestone, crushing the bauxite and limestone to a particle size of ≤88 mesh, and mixing them in a sand mixer to obtain a first mixed material;

[0122] S2, pressing the mixed material into a green body at a pressure of 150 MPa through a ball press;

[0123] S3, keeping the green body at 1400° C. for 2 h and sintering it to obtain an aluminum-silicon-calcium composite material;

[0124] The mass percentages of the components of the aluminum-silicon-calcium composite material are Al2O3:SiO2:CaO=37.6%:42.3%:20.1%; the relative density is 27.1% and the apparent porosity is 70.3%.

[0125] Figure 3 This is the XRD diagram of the aluminum-silicon-calcium composite material of Example 1 of the present invention. Figure 3 It is concluded that the phase composition of the aluminum-silicon-calcium composite material of Example 1 of the present invention is a corundum phase, namely Al2O3, a mullite phase, namely A3S2, and anorthite phase, namely CAS2.

[0126] Figure 4 This is a microstructure photo of the aluminum-silicon-calcium composite material of Example 1 of the present invention. Figure 4 Combined with Figure 3 , which further verified the analysis conclusion of XRD and explained that the aluminum-silicon-calcium material with microscopic crystal phase composition of corundum phase, i.e. Al2O3, mullite phase, i.e. A3S2, and calcium feldspar phase, i.e. CAS2 was successfully prepared.

[0127] Figure 5 This is a microstructure photo of the aluminum-silicon-calcium composite material of Comparative Example 1 of the present invention. Figure 4 and Figure 5 It can be seen that the microstructure consists of corundum phase, i.e. Al2O3, mullite phase, i.e. A3S2, and calcium feldspar phase, i.e. CAS2, an aluminum-silicon-calcium composite material interlaced with each other was observed, but the microstructure of the sample prepared without additives had more pores and the structure between the crystal phases was loose; the microstructure of the sample prepared by introducing additives was denser, and the structure between the crystal phases was more closely connected.

[0128] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. An aluminum-silicon-calcium composite material, characterized in that: The aluminum-silicon-calcium composite material consists of the following chemical components in mass percentage: Al2O3 36.7%-78.8%, SiO2 14.3%-42.7%, CaO 0.2%-20.6% and TiO2 1.0%-3.0%, and the sum of the mass percentages of the chemical components is 100%.

2. The aluminum-silicon-calcium composite material according to claim 1, characterized in that: The aluminum-silicon-calcium composite material is composed of the following raw materials in percentage by mass: Al2O3 39.8% to 76.7%, SiO2 15.6% to 39.6%, CaO 1.0% to 18.6% and TiO2 2.0% to 3.0%.

3. The aluminum-silicon-calcium composite material according to claim 1, characterized in that: The relative density of the aluminum-silicon-calcium composite material is 90.1% to 92.7%.

4. The aluminum-silicon-calcium composite material according to claim 1, characterized in that: The apparent porosity of the aluminum-silicon-calcium composite material is 3.2% to 4.9%.

5. A method for preparing an aluminum-silicon-calcium composite material according to any one of claims 1 to 4, characterized in that: The following steps are involved: Using bauxite and limestone as raw materials, crushing the bauxite and limestone and mixing them to obtain a first mixed material; Using TiO2 as a sintering aid, mixing the sintering aid with the first mixed material and then pressing to obtain a green body; The green body is sintered to obtain an aluminum-silicon-calcium composite material.

6. The method for preparing an aluminum-silicon-calcium composite material according to claim 5, characterized in that: The mass of the bauxite accounts for 75% to 99% of the total mass of the first mixed material.

7. The method for preparing an aluminum-silicon-calcium composite material according to claim 5, characterized in that: In the first mixed material, the particle sizes of bauxite and limestone are both ≤88 mesh.

8. The method for preparing an aluminum-silicon-calcium composite material according to claim 5, characterized in that: The purity of the TiO2 is ≥98.0%, and the particle size is ≤10 μm.

9. The method for preparing an aluminum-silicon-calcium composite material according to claim 5, wherein the mass ratio of TiO2 to the first mixed material is 1 to 3:

100.

10. The method for preparing an aluminum-silicon-calcium composite material according to claim 5, characterized in that: The sintering temperature is 1400° C. to 1500° C., and the sintering time is 2 h to 3 h.

Citation Information

Patent Citations

  • Anorthite-mullite complex-phase high-temperature resistant material and preparation method thereof

    CN102603313A

  • Method for preparing chamotte by adopting middle-low bauxite with low ratio of calcium to aluminum in lime sintering way

    CN104591242A

  • Mullite-anorthite-corundum multiphase microporous thermal insulation material and preparation method thereof

    CN107973619A

  • Preparation method of compact calcium dialuminate refractory clinker

    CN109456069A

  • Crystallized Silicate Powder by Synthesized and High Strengthened Porcelain body Having the Same

    KR1020150130725A