In-situ synthesis YAG phase reinforced AlON ceramic material and preparation method thereof

By regulating the generation and uniform distribution of YAG liquid phase in AlON ceramic preparation, the problems of complex preparation process, high cost and poor mechanical properties of AlON ceramic materials in the prior art are solved, and high density and mechanical properties are achieved. promote.

CN118930277AActive Publication Date: 2024-11-12BEIJING INST OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411206631.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The existing AlON ceramic material preparation process has problems such as complex process, high cost, low production efficiency, high sintering temperature and long insulation time, resulting in large grain size and poor mechanical properties. It is difficult to evenly distribute the sintering additives, which affects the performance of the final product.

Method used

By accurately controlling the SPS process, the Y2O3 sintering additive reacts with Al2O3 to form a YAG liquid phase, and is uniformly distributed during the sintering process, reducing the reaction temperature of Al2O3 and AlN, accelerating the density process, inhibiting grain growth, and at the end of sintering stage, The YAG liquid phase is made to dissolve in AlON ceramics to improve mechanical properties.

Benefits of technology

It realizes the rapid preparation of high-density AlON ceramics at lower sintering temperatures, significantly inhibits grain growth, enhances the fine crystal strengthening effect and solid solution strengthening effect of the material, and significantly improves the mechanical properties of the ceramics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930277A_ABST
    Figure CN118930277A_ABST
Patent Text Reader

Abstract

The invention discloses an in-situ synthesis YAG phase reinforced AlON ceramic material and a preparation method thereof. According to the method, Al2O3 and AlN are taken as raw materials, Y2O3 is taken as an auxiliary agent, and the high-performance AlON ceramic is successfully prepared by adopting a three-stage SPS process. A YAG liquid phase is generated in a ceramic preparation process through precise regulation and control of a sintering process, and the liquid phase is ensured to be uniformly distributed in gaps of powder particles and is completely dissolved in a ceramic matrix in a solid state at the final stage of sintering through further optimization of the process. The introduction of the YAG liquid phase significantly reduces the reaction temperature of Al2O3 and AlN, accelerates the densification of the material, and initiates the fine grain strengthening effect. Meanwhile, the YAG liquid phase is dissolved in a ceramic matrix in a solid solution mode in the later stage of sintering, and the solid solution strengthening effect is triggered. While the mechanical property of the AlON ceramic is remarkably improved, the low-temperature rapid preparation of the material is realized, the energy consumption and the production cost are reduced, and the method has a wide industrial application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an in-situ self-generated YAG phase reinforced AlON ceramic material and a preparation method thereof, belonging to the field of ceramic material preparation. Background Art

[0002] Aluminum oxynitride (AlON) ceramics have great application potential in the fields of police explosion protection, safety gear, high-pressure sodium lamps, special instrument manufacturing, etc. due to their high hardness, high strength, excellent wear resistance, good corrosion resistance and oxidation resistance, and excellent optical transparency (covering the near-ultraviolet to mid-infrared bands). It is also one of the ideal materials for the preparation of transparent armor and infrared windows.

[0003] At present, the mainstream method for preparing AlON ceramics is a two-step method, that is, first synthesizing AlON powder, and then obtaining AlON ceramics by high-temperature densification sintering. The common sintering method is pressureless sintering, and its sintering temperature is usually above 1800°C. Patent CN112299861A synthesizes pure phase AlON powder by traditional carbon thermal reduction nitridation method. After the powder is ball-milled and refined, a certain amount of γ-Al2O3 is added and mixed evenly, and AlON ceramic green body is prepared by dry pressing, and then kept at 1880°C for 8h for pressureless sintering to obtain AlON ceramics. Patent CN109516813A discloses a method for preparing highly translucent AlON ceramics by direct water injection molding. This method disperses pure phase AlON powder in deionized water containing a dispersant to prepare a slurry, and then prepares a green body by slip injection molding, and finally performs pressureless sintering at 1850-1900°C and 1.5-8h in a carbon furnace to obtain AlON ceramics. Patent CN113135759A discloses a method for preparing AlON ceramic powder by solution combustion synthesis, and performs pressureless sintering at 1800-2000°C for 1-20h to prepare AlON ceramics. However, these methods generally have the disadvantages of complex process, high cost, low production efficiency, etc., and due to the limitations of factors such as excessively high sintering temperature and long insulation time during the preparation process, the ceramic grain size is large and the mechanical properties are poor, which cannot meet the actual application requirements. In order to obtain high-quality AlON ceramics, sintering aids are usually required to be added during its preparation process, but due to the small amount of sintering aids added, the problem of uniform distribution in the ceramic matrix is ​​difficult to solve, thereby affecting the performance of the final product. In addition, the effect of the sintering aid is closely related to the sintering process of AlON ceramics.

[0004] In recent years, spark plasma sintering (SPS) technology has gradually become an important method for preparing high-performance ceramic materials due to its advantages such as fast heating rate, short sintering time, low sintering temperature, rapid cooling, energy saving and environmental protection. Compared with traditional pressureless sintering, hot pressing sintering and hot isostatic pressing sintering, SPS technology can achieve the preparation of high-density ceramic materials at a lower temperature and has better microstructure control capabilities. Although SPS technology has shown significant potential in reducing sintering temperature and inhibiting grain growth, how to further optimize the SPS process flow and parameters to meet the preparation requirements of AlON ceramics under specific sintering aid conditions is still a technical problem that needs to be solved urgently. Summary of the invention

[0005] The present invention aims to provide an in-situ self-generated YAG phase reinforced AlON ceramic material and a preparation method thereof, so as to overcome the deficiencies in the prior art. By precisely controlling the SPS process, the Y2O3 sintering aid reacts with Al2O3 during the sintering process to generate a YAG liquid phase, and ensures that the liquid phase is evenly distributed between the powder particles. The introduction of the YAG liquid phase significantly reduces the reaction temperature of Al2O3 and AlN, accelerates the densification process of the AlON ceramic, and enables it to be successfully prepared at a lower sintering temperature, thereby effectively inhibiting grain growth and significantly enhancing the fine grain strengthening effect of the material. At the same time, the YAG liquid phase is dissolved into the AlON ceramic at the end of sintering, further triggering the solid solution strengthening effect, and significantly improving the mechanical properties of the AlON ceramic.

[0006] The present invention provides a method for preparing an in-situ self-generated YAG phase reinforced AlON ceramic material, which mainly comprises the following steps:

[0007] Step 1) Selecting Al2O3 powder and AlN powder with a purity greater than 99% and a particle size range of 20 to 500 nm as raw materials, the mass ratio of the two is 0.79:0.21;

[0008] Step 2) adding Y2O3 with a purity greater than 99% and a particle size range of 10 to 100 nm as a single sintering aid, with a content of 0.2 wt% to 2 wt%;

[0009] Step 3) Put the raw material powder and sintering aid into a ball mill together, and mix and disperse the powder by using a forward and reverse alternating ball milling process. The ball mill speed is 100-400r / min, the ball mill time is 5-30h, and the ball mill direction is changed every 30min;

[0010] Step 4) loading the uniformly dispersed mixed powder or compact into a carbon-carbon mold;

[0011] Step 5) Place the assembled mold into the SPS furnace chamber for vacuum sintering to prepare AlON ceramics. The SPS sintering process is divided into three stages. In the first stage, a faster heating rate is used to increase the temperature to a predetermined value to ensure the smooth generation of the YAG liquid phase; in the second stage, while maintaining the temperature of the first stage, pressure is applied to the sintered body at a certain pressurization rate to ensure that the YAG liquid phase is evenly distributed in the gaps between the powder particles; in the third stage, the temperature and pressure are further increased to a predetermined value at a slower heating rate and a faster pressurization rate, and the temperature is kept for a certain period of time to ensure the smooth solid solution of the YAG liquid phase and finally obtain single-phase AlON ceramics. The specific sintering parameters are as follows: first, increase the temperature to 1200-1400°C at a heating rate of 150-300°C / min; then, while keeping the temperature unchanged, increase the pressure to 10-30MPa at a pressurization rate of 0.02-0.06MPa / s; finally, increase the temperature and pressure to 1500-1700°C and 50-100MPa, respectively, at a heating rate of 30-80°C / min and a pressurization rate of 0.1-0.3MPa / s, and keep warm for 5-20min.

[0012] The density of the in-situ self-generated YAG phase-reinforced AlON ceramic material is greater than 99.8%, and the hardness is greater than 17.5 GPa.

[0013] The beneficial effects of the present invention include:

[0014] (1) Through precise control of the SPS process, the YAG liquid phase was successfully generated and evenly distributed in the gaps between Al2O3 and AlN powder particles during the preparation of AlON ceramics. The introduction of the YAG liquid phase significantly reduced the reaction temperature of Al2O3 and AlN, accelerated the densification process of AlON ceramics, and thus achieved the rapid preparation of high-density AlON ceramics at a lower temperature, effectively inhibited grain growth, and caused the material to produce obvious fine grain strengthening. In the first stage of SPS sintering, a faster heating rate was used to quickly heat the material to the required temperature, which stimulated the sintering driving force, enhanced the diffusion on the surface of the powder particles, and improved the reaction activity, ensuring that the Y2O3 sintering aid reacted with the Al2O3 powder to generate the YAG liquid phase. In the second stage, by slowly applying pressure while keeping the temperature of the first stage unchanged, the generated YAG liquid phase was dispersed to the maximum extent and evenly distributed in the gaps between the powder particles. This process gave full play to the wettability and fluidity of the YAG liquid phase, promoted the rearrangement of the powder particles and the elimination of pores, and accelerated the densification process of the material. At the same time, it can greatly reduce the sintering activation energy of the powder, providing an effective guarantee for the decrease in the temperature of the solid-phase reaction between Al2O3 and AlN. During the third stage of sintering, on the basis of ensuring the uniform distribution of the liquid phase, the temperature and pressure are further increased to ensure the formation of the AlON phase. The slower heating rate in this stage helps to stabilize the thermal field, ensure the uniformity of the temperature inside the material, and avoid the occurrence of overburning and melting of AlON ceramics. At the same time, the slower heating rate provides sufficient time for the solid-phase reaction between Al2O3 and AlN, ensuring the complete reaction. The rapid pressurization process provides a strong mechanical driving force for the sintering of AlON ceramics, accelerates the densification process of the powder, and also promotes the solid solution of the YAG liquid phase, avoiding the residue of the second phase in the AlON ceramics.

[0015] (2) Due to the differences in lattice constants and ionic radii between YAG and AlON ceramics, when YAG is dissolved in AlON ceramics, it will cause lattice distortion, thereby increasing the internal stress of the material. In addition, the solid solution of YAG will also form local chemical inhomogeneities or atomic clusters in the lattice. These areas can act as obstacles to dislocation movement, hinder dislocation slip and increase dislocation density. These mechanisms work together to significantly improve the mechanical properties of AlON ceramics. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is the fracture morphology of the AlON ceramic after the first stage of SPS sintering in Example 1;

[0017] Figure 2 This is the fracture morphology of the AlON ceramic after the second stage of SPS sintering in Example 1;

[0018] Figure 3This is the fracture morphology of the AlON ceramic after the third stage of SPS sintering in Example 1;

[0019] Figure 4 This is the fracture morphology of the AlON ceramic after the first stage of SPS sintering in Example 2;

[0020] Figure 5 This is the fracture morphology of the AlON ceramic after the second stage SPS sintering in Example 2;

[0021] Figure 6 This is the fracture morphology of the AlON ceramic after the third stage of SPS sintering in Example 2;

[0022] Figure 7 This is the fracture morphology of the AlON ceramic after the first stage of SPS sintering in Example 3;

[0023] Figure 8 This is the fracture morphology of the AlON ceramic after the second stage of SPS sintering in Example 3;

[0024] Fig. 9 This is the fracture morphology of the AlON ceramic after the third stage of SPS sintering in Example 3; DETAILED DESCRIPTION

[0025] The present invention is further described below with reference to the accompanying drawings and specific embodiments, but they are not intended to limit the present invention.

[0026] Example 1

[0027] Step 1) Select Al2O3 and AlN powders with a purity of 99.99% and a particle size of 20 nm as raw materials, and the mass ratio of the two is 0.79:0.21;

[0028] Step 2) adding Y2O3 with a purity of 99.99% and a particle size of 10 nm as a sintering aid, the content of which is 2 wt%;

[0029] Step 3) Put the raw material powder and sintering aid into a ball mill together, and mix and disperse the powder by using a forward and reverse alternating ball milling process. The ball mill speed is 100r / min, the ball milling time is 30h, and the ball milling direction is changed every 30min;

[0030] Step 4) the mixed powder evenly dispersed after ball milling is loaded into a carbon-carbon mold, and the mold and the powder are separated by graphite paper;

[0031] Step 5) Place the assembled mold into the SPS furnace chamber for vacuum sintering to obtain AlON ceramics. The SPS sintering process adopts a three-stage sintering method. In the first stage of sintering, the temperature is raised to 1400°C at a heating rate of 300°C / min; in the second stage of sintering, while maintaining 1400°C, the pressure is raised to 30MPa at a pressurization rate of 0.06MPa / s; in the third stage of sintering, the temperature and pressure are raised to 1500°C and 100MPa, respectively, at a heating rate of 30°C / min and a pressurization rate of 0.3MPa / s, and kept warm for 20 minutes.

[0032] The AlON ceramics prepared in this example were tested, and the results were as follows:

[0033] (1) After the first stage of SPS sintering, the fracture morphology of AlON ceramics is as follows: Figure 1 It can be seen that although there is an obvious YAG liquid phase inside the sample (the white phase marked by the white dotted line), the liquid phase is not evenly dispersed in the gaps between the powder particles, and there is obvious agglomeration.

[0034] (2) After the second stage of SPS sintering, the fracture morphology of AlON ceramics is as follows: Figure 2 As shown in Figure 2, it can be seen that the YAG liquid phase is evenly distributed among the powder particles.

[0035] (3) After the third stage of SPS sintering, the fracture morphology of AlON ceramics is as follows: Figure 3 As shown in the figure, it can be seen that the overall structure of the ceramic is uniform and dense, and no YAG phase is found, indicating that YAG has been completely dissolved into the AlON ceramic.

[0036] (4) The density of the AlON ceramic in this embodiment is 99.91% and the hardness is 17.7 GPa.

[0037] Example 2

[0038] Step 1) Select Al2O3 and AlN powders with a purity of 99.99% and a particle size of 200 nm as raw materials, and the mass ratio of the two is 0.79:0.21;

[0039] Step 2) adding Y2O3 with a purity of 99.99% and a particle size of 50 nm as a sintering aid, the content of which is 1 wt%;

[0040] Step 3) Put the raw material powder and sintering aid into a ball mill together, and mix and disperse the powder by using a forward and reverse alternating ball milling process. The ball mill speed is 250r / min, the ball milling time is 20h, and the ball milling direction is changed every 30min;

[0041] Step 4) is the same as in Example 1;

[0042] Step 5) Place the assembled mold into the SPS furnace chamber for vacuum sintering to obtain AlON ceramics. The SPS sintering process adopts a three-stage sintering method. In the first stage of sintering, the temperature is raised to 1300°C at a heating rate of 200°C / min; in the second stage of sintering, while maintaining 1300°C, the pressure is raised to 20MPa at a pressurization rate of 0.04MPa / s; in the third stage of sintering, the temperature and pressure are raised to 1600°C and 75MPa, respectively, at a heating rate of 50°C / min and a pressurization rate of 0.2MPa / s, and kept warm for 10 minutes.

[0043] The AlON ceramics prepared in this example were tested, and the results were as follows:

[0044] (1) After the first stage of SPS sintering, the fracture morphology of AlON ceramics is as follows: Figure 4 It can be seen that although there is an obvious YAG liquid phase inside the sample (the white phase marked by the white dotted line), the liquid phase is not evenly dispersed in the gaps between the powder particles, and there is obvious agglomeration.

[0045] (2) After the second stage of SPS sintering, the fracture morphology of AlON ceramics is as follows: Figure 5 As shown in Figure 2, it can be seen that the YAG liquid phase is evenly distributed among the powder particles.

[0046] (3) After the third stage of SPS sintering, the fracture morphology of AlON ceramics is as follows: Figure 6 As shown in the figure, it can be seen that the overall structure of the ceramic is uniform and dense, and no YAG phase is found, indicating that YAG has been completely dissolved into the AlON ceramic.

[0047] (4) The density of the AlON ceramic in this embodiment is 99.89% and the hardness is 17.6 GPa.

[0048] Example 3

[0049] Step 1) Select Al2O3 and AlN powders with a purity of 99.99% and a particle size of 500 nm as raw materials, and the mass ratio of the two is 0.79:0.21;

[0050] Step 2) adding Y2O3 with a purity of 99.99% and a particle size of 100 nm as a sintering aid, with a content of 0.2 wt%;

[0051] Step 3) Put the raw material powder and sintering aid into a ball mill together, and mix and disperse the powder by using a forward and reverse alternating ball milling process. The ball mill speed is 400r / min, the ball milling time is 5h, and the ball milling direction is changed every 30min;

[0052] Step 4) is the same as in Example 1;

[0053] Step 5) Place the assembled mold into the SPS furnace chamber for vacuum sintering to obtain AlON ceramics. The SPS sintering process adopts a three-stage sintering method. In the first stage of sintering, the temperature is raised to 1200°C at a heating rate of 150°C / min; in the second stage of sintering, while maintaining 1200°C, the pressure is raised to 10MPa at a pressurization rate of 0.02MPa / s; in the third stage of sintering, the temperature and pressure are raised to 1700°C and 50MPa, respectively, at a heating rate of 80°C / min and a pressurization rate of 0.1MPa / s, and kept warm for 5 minutes.

[0054] The AlON ceramics prepared in this example were tested, and the results were as follows:

[0055] (1) After the first stage of SPS sintering, the fracture morphology of AlON ceramics is as follows: Figure 7 It can be seen that although there is an obvious YAG liquid phase inside the sample (the white phase marked by the white dotted line), the liquid phase is not evenly dispersed in the gaps between the powder particles, and there is obvious agglomeration.

[0056] (2) After the second stage of SPS sintering, the fracture morphology of AlON ceramics is as follows: Figure 8 As shown in Figure 2, it can be seen that the YAG liquid phase is evenly distributed among the powder particles.

[0057] (3) After the third stage of SPS sintering, the fracture morphology of AlON ceramics is as follows: Fig. 9 As shown in the figure, it can be seen that the overall structure of the ceramic is uniform and dense, and no YAG phase is found, indicating that YAG has been completely dissolved into the AlON ceramic.

[0058] (4) The density of the AlON ceramic in this embodiment is 99.90% and the hardness is 17.6 GPa.

[0059] The above content illustrates the embodiments of the present invention in conjunction with the accompanying drawings, but the present invention includes but is not limited to the above embodiments. Any modification, supplement, equivalent replacement or partial improvement made under the principle of the spirit of the present invention shall be deemed to be within the protection scope of the present invention.

Claims

1. A method for preparing an in-situ self-generated YAG phase reinforced AlON ceramic material, characterized in that: The process steps include: 1) Selecting nano-sized Al2O3 powder and AlN powder as raw materials; 2) Adding Y2O3 as a single sintering aid; 3) Put the raw material powder and the sintering aid into a ball mill, and use a ball mill to mix the powder; 4) loading the uniformly dispersed mixed powder or compact into a carbon-carbon mold after ball milling; 5) The assembled mold is placed in an SPS sintering furnace and sintered under vacuum conditions to obtain AlON ceramics.

2. The method for preparing the in-situ self-generated YAG phase reinforced AlON ceramic material according to claim 1, characterized in that: In the step 1), the purity of Al2O3 powder and AlN powder are both greater than 99%, the particle size range is 20-500nm, and the mass ratio of the two is 0.79:0.

21.

3. The method for preparing the in-situ self-generated YAG phase reinforced AlON ceramic material according to claim 1, characterized in that: In the step 2), the purity of the Y2O3 sintering aid is greater than 99%, the particle size range is 10 to 100 nm, and the added content is 0.2 to 2 wt%.

4. The method for preparing the in-situ self-generated YAG phase reinforced AlON ceramic material according to claim 1, characterized in that: In the step 3), the ball milling speed is 100-400 r / min, the ball milling time is 5-30 h, and the entire ball milling process is carried out alternately in forward and reverse directions, with the direction of rotation being changed every 30 minutes.

5. The method for preparing the in-situ self-generated YAG phase reinforced AlON ceramic material according to claim 1, characterized in that: In the step 5), the SPS sintering process adopts a three-stage sintering method. In the first stage of sintering, the temperature is raised to 1200-1400°C at a heating rate of 150-300°C / min; in the second stage of sintering, the pressure is raised to 10-30MPa at a pressurization rate of 0.02-0.06MPa / s while keeping the temperature unchanged; in the third stage of sintering, the temperature and pressure are raised to 1500-1700°C and 50-100MPa respectively at a heating rate of 30-80°C / min and a pressurization rate of 0.1-0.3MPa / s, and the temperature is kept for 5-20 minutes.

6. An in-situ self-generated YAG phase reinforced AlON ceramic material, characterized in that: Prepared by the method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Tape casting production method of large-size AlON transparent ceramic

    CN115636672A