Alumina porous ceramic substrate and preparation method thereof
The alumina porous ceramic substrate is prepared by ball milling, defoaming and casting of materials such as alumina powder and ball milling media, and calcining after static pressure, which solves the problem of using harmful crosslinking agents and insufficient thickness, and achieves high strength and thinness And environmentally friendly alumina porous ceramic substrate preparation.
Patent Information
- Application Number
- CN202411284790.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-12
AI Technical Summary
The existing methods for preparing alumina porous ceramic substrates use the harmful neurotoxic crosslinking agent acrylamide, and it is difficult to prepare a thin substrate while ensuring strength. The thicker the thickness, the worse the thermal conductivity.
Alumina powder, ball milling solvent, ball milling medium, starch, and dispersant mixed ball milling, and after defoaming, stalemate and casting, calcining the aluminum oxide porous ceramic substrate to avoid the use of toxic reagents and achieve high strength and thinness. Substrate preparation.
It realizes environmentally friendly aluminum oxide porous ceramic substrate preparation without toxic reagents, the process is simple and controllable, suitable for large-scale production, and improves the thickness and bending strength of the substrate.
Smart Images

Figure CN118930314A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alumina ceramic substrates, and specifically discloses an alumina porous ceramic substrate and a preparation method thereof. Background Art
[0002] Alumina porous ceramic substrates are made of alumina and have a unique porous structure. They have a large specific surface area and pore volume, and good mass and heat transfer performance. They also have excellent high-temperature stability and can withstand corrosion and oxidation in high-temperature environments. They can withstand corrosion and erosion from a variety of chemical media. They have good hardness and rigidity, and also have high compressive and bending strength. Based on the above advantages, alumina porous ceramic substrates are used in high-temperature filter materials, heat exchangers, calciner components, chemical reactors, catalyst carriers, etc., and can also be used in material processing, mechanical parts and structural parts.
[0003] At present, the main method for preparing porous alumina ceramic substrates is gel casting. First, alumina ceramic powder is added to a mixed solution of organic monomers and cross-linking agents to prepare a suspension, and then an initiator and a catalyst are added. The suspension is solidified and formed through the polymerization and cross-linking reaction of the organic monomers, and then sintered to prepare porous alumina ceramics. The advantage of gel casting is that it can be used to prepare porous alumina ceramics with complex shapes. The disadvantage is that the cross-linking agent acrylamide used in large quantities has strong neurotoxicity and is very harmful to the environment and the human body.
[0004] In addition, the thickness of alumina ceramic substrates generally ranges from 0.254mm to 4.0mm, including 0.254mm, 0.385mm, 1.0mm, 2.0mm, 3.0mm, 4.0mm and other specifications. The thickness of the substrate directly affects its strength, pressure resistance and thermal conductivity. The thicker the thickness, the better the strength and pressure resistance, but the thermal conductivity is relatively poor; on the contrary, although the thinner substrate has better thermal conductivity, its strength and pressure resistance are not as good as the thicker substrate. Generally speaking, the strength of a substrate with a thickness of about 1.00mm is about 34Mpa. How to prepare a thinner alumina ceramic substrate while ensuring the strength of the substrate is the focus of research and development. Summary of the invention
[0005] In view of the problems existing in the prior art, the main purpose of the present invention is to provide a method for preparing a high-strength and thin alumina porous ceramic substrate, and the preparation method is green and environmentally friendly.
[0006] To achieve the above objectives, the present invention provides the following specific technical solutions.
[0007] A method for preparing an alumina porous ceramic substrate comprises the following steps: (1) mixing and ball-milling alumina powder, a ball-milling solvent, a ball-milling medium, starch, and a dispersant to obtain a first mixed slurry; (2) adding a binder to the first mixed slurry and continuing ball milling to obtain a second mixed slurry; (3) performing degassing and aging treatment on the second mixed slurry to obtain a third mixed slurry; (4) tape casting the third mixed slurry to obtain a green body; (5) Static pressing of green compacts; (6) Calcine the green body after static pressing to obtain an alumina porous ceramic substrate.
[0008] In a further preferred embodiment, the ball milling solvent is at least one of anhydrous ethanol and methanol.
[0009] In a further preferred embodiment, the ball milling medium is a zirconia ball. Further preferably, the diameter of the zirconia ball is 5 to 25 mm.
[0010] In a further preferred embodiment, the dispersant is an alkyl aryl phosphate or an alkyl benzene sulfonate.
[0011] In a further preferred embodiment, the adhesive is acrylic polyester glue or polyurethane glue.
[0012] In a further preferred embodiment, in step (1) and step (2), the amount of alumina powder is 30-45%, the amount of ball milling solvent is 25-40%, the amount of dispersant is 0.5-1%, the amount of binder is 10-20%, and the amount of starch is 3-9%.
[0013] In a further preferred embodiment, the ball milling is performed in a ball mill. Further preferably, the ball milling speed in step (1) is 150-350 rpm, and the ball milling time is 10-14 h; the ball milling speed in step (2) is 200-400 rpm, and the ball milling time is 14-18 h.
[0014] In a further preferred embodiment, the degassing is vacuum degassing. Further preferably, the degassing is carried out in a degassing reactor. Further preferably, the degassing pressure is less than -0.1 MPa, and the degassing time is 30 to 60 min.
[0015] In a further preferred embodiment, the aging temperature is 20-26° C. and the aging time is 2-6 hours.
[0016] In a further preferred embodiment, a tape casting machine is used for tape casting, and further preferably, the temperature of the tape casting is 30-80° C., the speed of the tape casting is 0.2-0.5 m / min, and the height of the scraper is 1100-1500 μm.
[0017] In a further preferred embodiment, the method further comprises the step of vacuum sealing the green body before statically pressing the green body.
[0018] In a further preferred embodiment, the static pressure is 50-100 MPa, and the static pressure time is 30-60 min.
[0019] In a further preferred embodiment, the green body is statically pressed in a single piece, and the thickness of the green body after static pressing is 0.96-0.99 mm.
[0020] In a further preferred embodiment, the calcination is carried out in a combined calcination and discharge furnace.
[0021] In a further preferred embodiment, the calcination temperature is 1300-1600° C. and the calcination holding time is 4-7 hours.
[0022] In a further preferred embodiment, the heating rate of the calcination is 0.5-0.8°C / min.
[0023] Based on the same inventive concept, the present invention provides an alumina porous ceramic substrate prepared by the above preparation method.
[0024] The above one or more technical solutions of the present invention can achieve at least one of the following beneficial effects: The invention does not use toxic reagents and is environmentally friendly.
[0025] The preparation method provided by the invention has a short process, is simple and controllable, and is convenient for large-scale production.
[0026] The alumina porous ceramic substrate prepared by the present invention has a thickness of about 0.94-0.97 mm, but has relatively high strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is an electron microscope image of the porous alumina ceramic substrate obtained in Example 1.
[0028] Figure 2 This is an electron microscope image of the porous alumina ceramic substrate obtained in Example 2. DETAILED DESCRIPTION
[0029] Some embodiments of the present invention provide a method for preparing an alumina porous ceramic substrate, comprising the following steps: (1) mixing and ball-milling alumina powder, a ball-milling solvent, a ball-milling medium, starch, and a dispersant to obtain a first mixed slurry; (2) adding a binder to the first mixed slurry and continuing ball milling to obtain a second mixed slurry; (3) performing degassing and aging treatment on the second mixed slurry to obtain a third mixed slurry; (4) tape casting the third mixed slurry to obtain a green body; (5) Static pressing of green compacts; (6) Calcine the green body after static pressing to obtain an alumina porous ceramic substrate.
[0030] In some specific embodiments, the ball milling solvent is at least one of anhydrous ethanol and methanol.
[0031] In some specific embodiments, the ball milling medium is a zirconia ball. It is further preferred that the diameter of the zirconia ball is 5 to 25 mm.
[0032] In some specific embodiments, the dispersant is an alkyl aryl phosphate or an alkyl benzene sulfonate. More preferably, it is an alkyl benzene sulfonate, such as sodium dodecyl benzene sulfonate. The use of a dispersant to reduce the viscosity of solid particles is helpful for the molding operation of ceramic products.
[0033] In some specific embodiments, the adhesive is acrylic polyester glue or polyurethane glue, and polyurethane glue is more preferably used. Polyurethane glue contains isocyanate and carbamate groups with strong polarity and high chemical activity, and has excellent chemical adhesion with materials containing active hydrogen (such as foam plastics, ceramics and other porous materials). The hydrogen bonding effect between polyurethane and the bonded material will enhance the molecular cohesion, thereby making the bonding stronger.
[0034] In some specific embodiments, by weight percentage, in step (1) and step (2), the amount of alumina powder is 30-45%, the amount of ball milling solvent is 25-40%, the amount of dispersant is 0.5-1%, the amount of binder is 10-20%; and the amount of starch is 10-20% of the alumina powder.
[0035] In some specific embodiments, by weight percentage, in step (1) and step (2), the amount of alumina powder is 30-45%, the amount of methanol is 20-30%, the amount of anhydrous ethanol is 5-10%, the amount of dispersant is 0.5-1%, the amount of binder is 10-20%; and the amount of starch is 3-9%.
[0036] In some specific embodiments, the ball milling is performed in a ball mill.
[0037] In some specific embodiments, the ball milling speed in step (1) is 150-350 rpm, and the ball milling time is 10-14 h; the ball milling speed in step (2) is 200-400 rpm, and the ball milling time is 14-18 h.
[0038] In some specific embodiments, the degassing is vacuum degassing.
[0039] In some specific embodiments, degassing is performed in a degassing reactor. It is further preferred that the degassing pressure is less than -0.1Mpa, and the degassing time is 30 to 60 minutes. Vacuum degassing is mainly used to remove large bubbles in the slurry. The present invention uses vacuum degassing instead of chemical reagent degassing to avoid the introduction of impurities by chemical reagent degassing.
[0040] In some specific embodiments, the aging temperature is 20-26°C; the aging time is 2-6 hours. During the degassing process, it is a negative pressure state, the powder in the slurry moves upward, and the aging process is a relatively static state, so that the powder is fully and evenly distributed in the slurry.
[0041] In some specific embodiments, a tape casting machine is used for tape casting, and preferably the temperature of the tape casting is 30-80° C., the speed of the tape casting is 0.2-0.5 m / min, and the height of the scraper is 1100-1500 μm.
[0042] In some specific embodiments, the step of vacuum sealing the green body is further included before isostatic pressing the green body. Because the isostatic pressing process is heated and pressurized, the sample is placed in water, and the green body is vacuum sealed to prevent the green body from being affected by contact with water.
[0043] In some specific implementation methods, the static pressure is 50-100 MPa, and the static pressure time is 30-60 min.
[0044] In some specific embodiments, the green body is statically pressed as a single piece, and the thickness of the green body after static pressing is 0.96-0.99 mm.
[0045] In some specific embodiments, the calcination is carried out in a combined calcination and row furnace. Before calcination, the cooking bag sealing the green body is removed. In some specific embodiments, the calcination temperature is 1300-1600° C.; the calcination holding time is 4-7 hours.
[0046] In some specific embodiments, the heating rate of the calcination is 0.5-0.8°C / min.
[0047] In addition, some embodiments of the present invention show the prepared alumina porous ceramic substrate.
[0048] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0049] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0050] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0051] Example 1 Use a 15L ball mill, add 25% methanol, 10% anhydrous ethanol, and 1% dispersant sodium dodecylbenzene sulfonate in order by mass, stir thoroughly, add 40% alumina powder and 4% starch, then add 2kg of zirconium balls with diameters of 10mm, 15mm, and 20mm respectively, and ball mill at a speed of 300rpm for 12h; add 20% of the binder polyimide, and ball mill at a speed of 400rpm for 16h.
[0052] The ball-milled material was transferred to a 20L degassing reactor, and the degassing reactor was negatively pressurized to -0.1Mpa for degassing for 0.5h, with a stirring blade speed of 10Hz. The vacuum pump was turned off and aged for 2h, with a stirring blade speed of 5Hz, and the temperature in the reactor was always maintained at 22°C in a constant temperature water bath. After aging for 2 hours, open the valve to release the negative pressure, add positive pressure to the degassing reactor to 0.08Mpa, send the degassing and aged materials into the hopper of the tape casting machine for discharge, and use filters with precisions of 0.5μm and 1μm to filter impurities. The tape casting machine drying channel adopts a three-stage drying mode of 30℃, 45℃, and 60℃, opens the tape casting film belt, and casts at a speed of 0.2m / min. The scraper height is adjusted to 1300μm, and the green billet with a uniform thickness of 1000μm is discharged.
[0053] The green sheet after casting was collected, cut into sheets with a width of 200 mm, and dried at 150° C. for 6 h in a flat manner. The green sheet was taken out, cooled, and placed in a mold to be punched into a size of 185*185 mm.
[0054] The punched green pieces are placed in vacuum cooking bags, with each vacuum cooking bag only containing one green piece. The vacuum cooking bags are then evacuated and heat-sealed, and placed in a hydrostatic press in turn, and pressed at a pressure of 70 MPa for 40 minutes. The thickness of the green pieces after static pressing is 0.98 mm.
[0055] After isostatic pressing, the green body is removed from the cooking bag, stacked on a ceramic refractory support plate, and placed in a firing furnace. The highest temperature is set to 1500℃, and the temperature is raised from room temperature to 1500℃ at a rate of 0.8℃ / min, and kept at this temperature for 5 hours. After natural cooling, the porous alumina ceramic substrate is taken out of the furnace.
[0056] Figure 1 This is an electron microscope image of the obtained porous alumina ceramic substrate.
[0057] Example 2 Select a 15L ball mill, add 20% methanol, 8% anhydrous ethanol, and 0.5% dispersant sodium dodecylbenzene sulfonate in order by mass, add 45% alumina powder and 9% starch after sufficient stirring, then add 2kg of zirconium balls with diameters of 10mm, 15mm, and 25mm respectively, and ball mill at a speed of 350rpm for 10h; add 17.5% binder polyimide and ball mill at a speed of 300rpm for 16h.
[0058] The ball-milled material was transferred to a 20L degassing reactor, and the degassing reactor was negatively pressurized to -0.2Mpa for degassing for 0.5h, with a stirring blade speed of 10Hz. The vacuum pump was turned off and aged for 4h, with a stirring blade speed of 5Hz, and the temperature in the reactor was always maintained at 26°C in a constant temperature water bath. After aging for 4 hours, the valve is opened to release the negative pressure, and the degassing reactor is pressurized to 0.01Mpa. The degassing and aged materials are sent to the hopper of the tape casting machine for discharge, and impurities are filtered out using filters with precisions of 0.5μm and 1μm. The tape casting machine drying channel adopts a three-stage drying mode of 30℃, 45℃, and 60℃, and the tape casting film belt is turned on, and the casting is carried out at a speed of 0.4m / min. The scraper height is adjusted to 1500μm, and the green body with a uniform thickness of 1150μm is discharged.
[0059] The green sheet after casting was collected, cut into sheets with a width of 200 mm, and dried at 150° C. for 6 h in a flat manner. The green sheet was taken out, cooled, and placed in a mold to be punched into a size of 185*185 mm.
[0060] The punched green pieces are placed in vacuum cooking bags, with each vacuum cooking bag only containing one green piece. The vacuum cooking bags are then evacuated and heat-sealed, and placed in a hydrostatic press in turn, and pressed at a pressure of 100 MPa for 30 minutes. The thickness of the green pieces after static pressing is 0.96 mm.
[0061] After isostatic pressing, the green body is removed from the cooking bag, stacked on a ceramic refractory support plate, and placed in a firing furnace. The highest temperature is set to 1300°C, and the temperature is raised from room temperature to 1300°C at a rate of 0.5°C / min, and kept at this temperature for 5 hours. After natural cooling, the porous alumina ceramic substrate is obtained.
[0062] Figure 2 This is an electron microscope image of the obtained porous alumina ceramic substrate.
[0063] Example 3 Select a 15L ball mill, add 30% methanol, 5% anhydrous ethanol, and 1% dispersant sodium dodecylbenzene sulfonate in order by mass, add 40% alumina powder and 6% starch after sufficient stirring, then add 2kg of zirconium balls with diameters of 10mm, 15mm, and 20mm respectively, and ball mill at a speed of 300rpm for 10h; add 18% binder polyimide and ball mill at a speed of 200rpm for 18h.
[0064] The ball-milled material was transferred to a 20L degassing reactor, and the degassing reactor was negatively pressurized to -0.1Mpa for degassing for 0.5h, with a stirring blade speed of 10Hz. The vacuum pump was turned off and aged for 6h, with a stirring blade speed of 5Hz, and the temperature in the reactor was always maintained at 20℃ in a constant temperature water bath. After aging for 6 hours, the valve is opened to release the negative pressure, and the degassing reactor is pressurized to 0.1Mpa. The degassing and aged materials are sent to the hopper of the tape casting machine for discharge, and impurities are filtered out using filters with precisions of 0.5μm and 1μm. The tape casting machine drying channel adopts a three-stage drying mode of 30℃, 45℃, and 60℃, and the tape casting film belt is turned on, and the casting is carried out at a speed of 0.3m / min. The scraper height is adjusted to 1100μm, and the green billet with a uniform thickness of 850μm is discharged.
[0065] The green sheet after casting was collected, cut into sheets with a width of 200 mm, and dried at 150° C. for 6 h in a flat manner. The green sheet was taken out, cooled, and placed in a mold to be punched into a size of 185*185 mm.
[0066] The punched green pieces are placed in vacuum cooking bags, with each vacuum cooking bag only containing one green piece. The vacuum cooking bags are then evacuated and heat-sealed, and placed in a hydrostatic press in turn, and pressed at a pressure of 50 MPa for 60 minutes. The thickness of the green pieces after static pressing is 0.99 mm.
[0067] After isostatic pressing, the green body is removed from the vacuum cooking bag, stacked on a ceramic refractory support plate, and placed in a firing furnace. The highest temperature is set to 1600°C, and the temperature is raised from room temperature to 1600°C at a rate of 0.5°C / min, and kept at this temperature for 7 hours. After natural cooling, the porous alumina ceramic substrate is obtained.
[0068] Example 4 Select a 15L ball mill, add 30% methanol, 10% anhydrous ethanol, and 1% dispersant sodium dodecylbenzene sulfonate in order by mass, add 35% alumina powder and 8% starch after sufficient stirring, then add 2kg of zirconium balls with diameters of 10mm, 15mm, and 20mm respectively, and ball mill at a speed of 150rpm for 14h; add 16% binder polyimide and ball mill at a speed of 400rpm for 16h.
[0069] The ball-milled material was transferred to a 20L degassing reactor, and the degassing reactor was negatively pressurized to -0.1Mpa for degassing for 0.5h, with a stirring blade speed of 10Hz. The vacuum pump was turned off and aged for 2h, with a stirring blade speed of 5Hz, and the temperature in the reactor was always maintained at 22°C in a constant temperature water bath. After aging for 2 hours, open the valve to release the negative pressure, add positive pressure to the degassing reactor to 0.08Mpa, send the degassing and aged materials into the hopper of the tape casting machine for discharge, and use filters with precision of 0.5μm and 1μm to filter impurities. The tape casting machine drying channel adopts a three-stage drying mode of 30℃, 45℃, and 60℃, opens the tape casting film belt, and casts at a speed of 0.2m / min. The scraper height is adjusted to 1300μm, and the green body with uniform thickness of 1000μm is discharged.
[0070] The green sheet after casting was collected, cut into sheets with a width of 200 mm, and dried at 150° C. for 6 h in a flat manner. The green sheet was taken out, cooled, and placed in a mold to be punched into a size of 185*185 mm.
[0071] The punched green pieces are placed in vacuum cooking bags, with each vacuum cooking bag only containing one green piece. The vacuum cooking bags are then evacuated and heat-sealed, and placed in a hydrostatic press in turn, and pressed at a pressure of 80 MPa for 40 minutes. The thickness of the green pieces after static pressing is 0.97 mm.
[0072] The green body after isostatic pressing is stacked on a ceramic refractory support plate in a stacking manner, and placed in a firing furnace. The highest temperature of the program is set to 1400°C, and the temperature is raised from room temperature to 1400°C at a rate of 0.5°C / min, and kept at this temperature for 4 hours. After natural cooling, the porous alumina ceramic substrate is taken out of the furnace.
[0073] The flexural strength of the porous alumina ceramic substrates obtained in Examples 1-4 was tested in the following manner: GB / T39826-2021, four-point bending method.
[0074] The porosity of the porous alumina ceramic substrates obtained in Examples 1-4 was tested in the following manner: GB / T 1966-2024, Determination of apparent porosity and bulk density of porous ceramics.
[0075] The test results are as follows: Table 1 From the data in Table 1, it can be seen that the porous alumina ceramic substrate obtained in Example 1 has a thickness of 0.96 mm and a porosity of 62.8%, but has a flexural strength of 56 MPa, achieving the goal of ensuring the flexural strength. In other embodiments, the thickness of the substrate is further reduced. The bending strength of the substrate is improved. In general, the alumina porous ceramic substrate provided by the present invention The preparation method can obtain a thin alumina porous ceramic substrate with high bending strength.
[0076] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing an alumina porous ceramic substrate, It is characterized in that The following steps are involved: (1) mixing and ball-milling alumina powder, a ball-milling solvent, a ball-milling medium, starch, and a dispersant to obtain a first mixed slurry; (2) adding a binder to the first mixed slurry and continuing ball milling to obtain a second mixed slurry; (3) performing degassing and aging treatment on the second mixed slurry to obtain a third mixed slurry; (4) tape casting the third mixed slurry to obtain a green body; (5) Static pressing of green compacts; (6) Calcine the green body after static pressing to obtain an alumina porous ceramic substrate.
2. The method for preparing the porous alumina ceramic substrate according to claim 1, It is characterized in that The ball milling solvent is at least one of anhydrous ethanol and methanol; the ball milling medium is zirconia balls; and the diameter of the zirconia balls is 5-25 mm.
3. The method for preparing the porous alumina ceramic substrate according to claim 1, It is characterized in that The dispersant is alkyl aryl phosphate or alkyl benzene sulfonate; the binder is acrylic polyester glue or polyurethane glue.
4. The method for preparing the porous alumina ceramic substrate according to any one of claims 1 to 3, It is characterized in that In terms of weight percentage, in step (1) and step (2), the amount of alumina powder is 30-45%, the amount of ball milling solvent is 25-40%, the amount of dispersant is 0.5-1%, the amount of binder is 10-20%, and the amount of starch is 3-9%.
5. The method for preparing the porous alumina ceramic substrate according to any one of claims 1 to 3, It is characterized in that Ball milling in a ball mill; in step (1), the speed of the ball milling is 150-350 rpm, and the ball milling time is 10-14 h; in step (2), the speed of the ball milling is 200-400 rpm, and the ball milling time is 14-18 h.
6. The method for preparing the porous alumina ceramic substrate according to any one of claims 1 to 3, It is characterized in that The degassing is vacuum degassing; the aging temperature is 20-26° C.; and the aging time is 2-6 hours.
7. The method for preparing the porous alumina ceramic substrate according to any one of claims 1 to 3, It is characterized in that The tape casting machine is used for tape casting; the temperature of the tape casting is 30-80°C, the speed of the process molding is 0.2-0.5m / min, and the scraper height is 1100-1500μm.
8. The method for preparing the alumina porous ceramic substrate according to any one of claims 1 to 3, It is characterized in that The static pressing pressure is 50-100 MPa, and the static pressing time is 30-60 min. The green body is statically pressed alone, and the thickness of the green body after static pressing is 0.96-0.99 mm.
9. The method for preparing the porous alumina ceramic substrate according to any one of claims 1 to 3, It is characterized in that The calcination temperature is 1300-1600° C.; the calcination holding time is 4-7 hours; and the calcination heating rate is 0.5-0.8° C. / min.
10. Alumina porous ceramic substrate, It is characterized in that It is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Porous ceramic radiating fin and preparation method
CN103910535A
Large-size ceramic substrate, and preparation method and production line thereof
CN105906331A
Preparation method and application of aluminium oxide ceramics
CN108516806A
Porous alumina ceramic plate, and preparation method thereof
CN110330358A
Flexible ceramic current collecting layer film green body
CN110981527A
Cited By
Novel lightweight high-temperature-resistant high-purity aluminum oxide and preparation method thereof
CN121248318A