High-temperature co-fired ceramic printing paste and preparation method thereof

Through the high-temperature co-fired ceramic printing paste composed of tungsten powder, inorganic bonding phase and organic carrier, the problem of sintering matching between the conductive paste and the substrate is solved, and the stability and consistency of the high-temperature co-fired ceramic is achieved, and inconsistent shrinkage is avoided. and warping defects improve the structural and conductive properties of ceramic circuit boards.

CN118930322APending Publication Date: 2024-11-12JUNYUAN ELECTRONIC TECHNOLOGY (HAINING) CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410821831.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In high-temperature co-fired ceramic technology, the matching problem between the conductive paste and the substrate sintering process leads to inconsistency in shrinkage and warping defects, making it difficult to achieve the stability and consistency of high-temperature co-fired ceramics.

Method used

High-temperature co-fired ceramic printing paste composed of tungsten powder, inorganic bonding phase and organic carrier are prepared by ball milling and homogenizer stirring, combining SiO2 and CaCO3 as sintering aids to ensure the particle size distribution and mixing of tungsten powder. Uniformity, forming a metallized slurry with good fluidity and thixotropy, and is suitable for co-firing with high temperature matching of alumina substrates.

Benefits of technology

The high-temperature co-fired ceramic printing paste is achieved with good fluidity and thixotropy, ensuring high-temperature matching with the alumina substrate, avoiding shrinkage inconsistency and warping, and improving the structural stability and conductive properties of the ceramic circuit board.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses high-temperature co-fired ceramic printing paste and a preparation method thereof, and belongs to the technical field of ceramic sintering, the high-temperature co-fired ceramic printing paste comprises the following components: 80-90 wt% of tungsten powder, 0-5.0 wt% of an inorganic binding phase, and 8-15 wt% of an organic carrier. The preparation method comprises the steps that a certain number of ball-milling beads are put into a ball-milling tank, then tungsten powder and an inorganic binding phase are put into the ball-milling tank to be subjected to dry milling, after ball milling is finished, the ball-milling beads and metallized powder are separated, and a mixture of the tungsten powder and inorganic phase powder is obtained; heating the solvent in the organic carrier in a water bath kettle at 60-80 DEG C, and then adding the thickening agent while stirring until the thickening agent is completely dissolved; the preparation method comprises the following steps: mixing a mixture of tungsten powder and inorganic phase powder with an organic carrier, stirring in a homogenizer to obtain mixed tungsten slurry, and grinding the rapidly stirred mixed slurry for multiple times by using a three-roller machine to obtain the required metallized tungsten slurry for multilayer aluminum oxide ceramics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic sintering, and in particular to a high-temperature co-fired ceramic printing slurry and a preparation method thereof. Background Art

[0002] High temperature co-fired ceramic (HTCC) is a multilayer ceramic circuit board made by screen printing conductive paste on a ceramic substrate according to circuit design requirements. HTCC has the characteristics of high structural strength, good thermal conductivity, good chemical stability, high wiring density, etc., and has broad application prospects in high-power micro-assembly circuits. Alumina and aluminum nitride ceramics are widely used as HTCC substrates for electronic devices. Alumina ceramics, as the most mature ceramic substrate material, have many advantages, such as low dielectric loss, excellent mechanical strength, and low preparation cost.

[0003] The firing temperature of the HTCC process is generally greater than 1500°C. Due to the high firing temperature, HTCC cannot use low melting point metal materials such as gold, silver, and copper, but must use refractory metal materials such as tungsten, molybdenum, and manganese. The melting point of metal tungsten is as high as 3410°C and has good electrical conductivity.

[0004] The most critical problem in the application of conductive paste in HTCC technology is the matching problem of co-firing. The sintering process of the conductive paste should match the sintering process of the substrate. In the sintering process of high-temperature co-fired ceramics, defects such as inconsistent shrinkage and warping occur. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a high-temperature co-fired ceramic printing slurry and a preparation method thereof, which has good fluidity and thixotropy, and can be co-fired with an alumina substrate at a high temperature, has consistent shrinkage, and has no warping.

[0006] In order to solve the above technical problems, the technical solution of the present invention is:

[0007] In one aspect, the present invention provides a high temperature co-fired ceramic printing paste, comprising the following components:

[0008] Tungsten powder: 80-90wt%, inorganic binder phase: 0-5.0wt%, organic carrier: 8-15wt%.

[0009] Preferably, the tungsten powder is spherical particles, the particle sizes of the spherical particles are 1-2 μm and 2-3 μm, and the weight ratio of the particle sizes of 1-2 μm to 2-3 μm is (60wt%-100wt%): (0wt%-40wt%).

[0010] Preferably, the inorganic binder phase comprises 95-99 wt% of powdered Al 2 O 3, and 1 to 5 wt% of a sintering aid.

[0011] Preferably, the composition of the sintering aid includes: 1wt% to 3wt% SiO 2 and 1 wt% to 2 wt% CaCO 3 .

[0012] Preferably, the organic vehicle comprises 5 to 15 wt % of a thickener and 85 to 95 wt % of a solvent.

[0013] Preferably, the thickener is any one of methyl cellulose, ethyl cellulose, polyvinyl alcohol, polyvinyl butyral, polyvinyl acid, phenolic resin and epoxy resin, or a mixture of two or more thereof.

[0014] Preferably, the solvent is any one of methanol, ethanol, toluene, acetone, xylene, butyl acetate, terpineol and butyl carbitol, or a mixture of two or more thereof.

[0015] On the other hand, the present invention provides a method for preparing a high temperature co-fired ceramic printing paste, the method comprising the following steps:

[0016] Preparation of metallized powder: a certain number of ball milling beads are placed in a ball milling jar, and then tungsten powder and inorganic binder phase are placed in the ball milling jar for dry grinding. After the ball milling is completed, the ball milling beads and metallized powder are separated to obtain a mixture of tungsten powder and inorganic phase powder;

[0017] Preparation of organic carrier: Heat the solvent in the organic carrier in a water bath at 60-80°C, then add the thickener while stirring until the thickener is completely dissolved;

[0018] The preparation steps of the metallized tungsten slurry are as follows: tungsten powder, a mixture of inorganic phase powder and an organic carrier are mixed and placed in a homogenizer for stirring to obtain a mixed tungsten slurry, and the quickly stirred mixed slurry is ground multiple times with a three-roll mill to obtain the required metallized tungsten slurry for multi-layer alumina ceramics.

[0019] Preferably, the tungsten powder and the inorganic binder phase are ball-milled for 24 to 48 hours. After the ball-milling, the ball milling beads and the metallized powder are separated by a 300-mesh sieve.

[0020] Preferably, the stirring speed in the homogenizer is 1000-2000 rpm.

[0021] The above technical solution has the following beneficial effects:

[0022] The metallization slurry has good fluidity and thixotropy, and can be co-fired with the alumina substrate at high temperature, with consistent shrinkage and no warping. DETAILED DESCRIPTION

[0023] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0024] Example 1

[0025] High temperature co-fired ceramic printing paste, including the following components:

[0026] Tungsten powder: 85wt%, inorganic binder phase: 1wt%, organic carrier: 14wt%;

[0027] The tungsten powder is spherical particles, the particle sizes of the tungsten powder particles are 1-2 μm and 2-3 μm, and the weight ratio of the particle sizes of 1-2 μm and 2-3 μm is 60wt%:40wt%;

[0028] Inorganic binder phase includes: 98wt% Al 2 O 3 Powder, 1wt% SiO 2 and 1wt% CaCO 3 ;

[0029] The organic carrier comprises: 5wt% of ethyl cellulose and 95wt% of pinene alcohol;

[0030] In other implementations of this embodiment, ethyl cellulose can be replaced by any one of methyl cellulose, polyvinyl alcohol, polyvinyl butyrate, polyvinyl acid, phenolic resin and epoxy resin, or a mixture of two or more thereof;

[0031] In other implementations of this embodiment, terpineol can be replaced by any one of methanol, ethanol, toluene, acetone, xylene, butyl acetate and butyl carbitol, or a mixture of two or more thereof;

[0032] The metallized tungsten slurry obtained above was printed on the surface of an alumina green body with a thickness of 300 mm and a size of 200 × 200 mm, and then dried and placed in a sintering furnace at a sintering temperature of 1500-1600°C for 3-4 hours. After sintering, multiple points of the printed surface, for example 40-50 points, were taken and the film thickness and roughness of the printed surface of the alumina substrate were tested using a desktop roughness meter. After testing, the film thickness of the printed surface was about 0.2 μm and the roughness was 0.5-0.65 μm.

[0033] Example 2

[0034] High temperature co-fired ceramic printing paste, including the following components:

[0035] Tungsten powder: 88wt%, inorganic binder phase: 2wt%, organic carrier: 10wt%;

[0036] The tungsten powder is spherical particles, the particle sizes of the tungsten powder particles are 1-2 μm and 2-3 μm, and the weight ratio of the particle sizes of 1-2 μm and 2-3 μm is 70wt%:30wt%;

[0037] Inorganic binder phase includes: 97.5wt% Al 2 O 3 Powder, 1wt% SiO 2 and 1.5wt% CaCO 3 ;

[0038] The organic carrier comprises: 10 wt % of ethyl cellulose and 90 wt % of pinene alcohol;

[0039] In other implementations of this embodiment, ethyl cellulose can be replaced by any one of methyl cellulose, polyvinyl alcohol, polyvinyl butyrate, polyvinyl acid, phenolic resin and epoxy resin, or a mixture of two or more thereof;

[0040] In other implementations of this embodiment, terpineol can be replaced by any one of methanol, ethanol, toluene, acetone, xylene, butyl acetate and butyl carbitol, or a mixture of two or more thereof;

[0041] The metallized tungsten slurry obtained above was printed on the surface of an alumina green body with a thickness of 300 mm and a size of 200 × 200 mm, and then dried and placed in a sintering furnace at a sintering temperature of 1500-1600°C for 3-4 hours. After sintering, multiple points of the printed surface, for example 40-50 points, were taken and the film thickness and roughness of the printed surface of the alumina substrate were tested using a desktop roughness meter. After testing, the film thickness of the printed surface was about 0.2 μm and the roughness was 0.5-0.65 μm.

[0042] Example 3

[0043] High temperature co-fired ceramic printing paste, including the following components:

[0044] Tungsten powder: 90wt%, inorganic binder phase: 2wt%, organic carrier: 8wt%;

[0045] The tungsten powder is spherical particles, the particle sizes of the tungsten powder particles are 1-2 μm and 2-3 μm, and the weight ratio of the particle sizes of 1-2 μm and 2-3 μm is 80wt%:20wt%;

[0046] Inorganic binder phase includes: 96.5wt% Al 2 O 3Powder, 1.5wt% SiO 2 and 2wt% CaCO 3 ;

[0047] The organic carrier comprises: 15 wt % of ethyl cellulose and 85 wt % of pinene alcohol;

[0048] In other implementations of this embodiment, ethyl cellulose can be replaced by any one of methyl cellulose, polyvinyl alcohol, polyvinyl butyrate, polyvinyl acid, phenolic resin and epoxy resin, or a mixture of two or more thereof;

[0049] In other implementations of this embodiment, terpineol can be replaced by any one of methanol, ethanol, toluene, acetone, xylene, butyl acetate and butyl carbitol, or a mixture of two or more thereof;

[0050] The metallized tungsten slurry obtained above was printed on the surface of an alumina green body with a thickness of 300 mm and a size of 200 × 200 mm, and then dried and placed in a sintering furnace at a sintering temperature of 1500-1600°C for 3-4 hours. After sintering, multiple points of the printed surface, for example 40-50 points, were taken and the film thickness and roughness of the printed surface of the alumina substrate were tested using a desktop roughness meter. After testing, the film thickness of the printed surface was about 0.2 μm and the roughness was 0.5-0.65 μm.

[0051] Example 4

[0052] High temperature co-fired ceramic printing paste, including the following components:

[0053] Tungsten powder: 80wt%, inorganic binder phase: 0wt%, organic carrier: 8wt%;

[0054] The tungsten powder is spherical particles, the particle sizes of the tungsten powder particles are 1-2 μm and 2-3 μm, and the weight ratio of the particle sizes of 1-2 μm and 2-3 μm is 60wt%:0wt%;

[0055] Inorganic binder phase includes: 95wt% Al 2 O 3 Powder, 1wt% SiO 2 and 1wt% CaCO 3 ;

[0056] The organic carrier comprises: 5wt% of ethyl cellulose and 85wt% of pinene alcohol;

[0057] In other implementations of this embodiment, ethyl cellulose can be replaced by any one of methyl cellulose, polyvinyl alcohol, polyvinyl butyrate, polyvinyl acid, phenolic resin and epoxy resin, or a mixture of two or more thereof;

[0058] In other implementations of this embodiment, terpineol can be replaced by any one of methanol, ethanol, toluene, acetone, xylene, butyl acetate and butyl carbitol, or a mixture of two or more thereof;

[0059] The metallized tungsten slurry obtained above was printed on the surface of an alumina green body with a thickness of 300 mm and a size of 200 × 200 mm, and then dried and placed in a sintering furnace at a sintering temperature of 1500-1600°C for 3-4 hours. After sintering, multiple points of the printed surface, for example 40-50 points, were taken and the film thickness and roughness of the printed surface of the alumina substrate were tested using a desktop roughness meter. After testing, the film thickness of the printed surface was about 0.2 μm and the roughness was 0.5-0.65 μm.

[0060] Example 5

[0061] High temperature co-fired ceramic printing paste, including the following components:

[0062] Tungsten powder: 90wt%, inorganic binder phase: 5wt%, organic carrier: 15wt%;

[0063] The tungsten powder is spherical particles, the particle sizes of the tungsten powder particles are 1-2 μm and 2-3 μm, and the weight ratio of the particle sizes of 1-2 μm and 2-3 μm is 100wt%:40wt%;

[0064] Inorganic binder phase includes: 99wt% Al 2 O 3 Powder, 3wt% SiO 2 and 2wt% CaCO 3 ;

[0065] The organic carrier comprises: 15 wt % of ethyl cellulose and 95 wt % of pinene alcohol;

[0066] In other implementations of this embodiment, ethyl cellulose can be replaced by any one of methyl cellulose, polyvinyl alcohol, polyvinyl butyrate, polyvinyl acid, phenolic resin and epoxy resin, or a mixture of two or more thereof;

[0067] In other implementations of this embodiment, terpineol can be replaced by any one of methanol, ethanol, toluene, acetone, xylene, butyl acetate and butyl carbitol, or a mixture of two or more thereof;

[0068] The metallized tungsten slurry obtained above was printed on the surface of an alumina green body with a thickness of 300 mm and a size of 200 x 200 mm. After drying, it was placed in a sintering furnace at a sintering temperature of 1500-1600°C and a sintering time of 3-4 hours. After sintering, multiple points of the printed surface, for example 40-50 points, were taken and the film thickness and roughness of the printed surface of the alumina substrate were tested using a desktop roughness meter. After testing, the film thickness of the printed surface was about 0.2 μm and the roughness was 0.5-0.65 μm, which met the requirements.

[0069] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. A high temperature co-fired ceramic printing paste, characterized in that: Includes the following components: Tungsten powder: 80-90wt%, inorganic binder phase: 0-5.0wt%, organic carrier: 8-15wt%.

2. The high temperature co-fired ceramic printing paste according to claim 1, characterized in that: The tungsten powder is spherical particles, the particle sizes of the spherical particles are 1-2 μm and 2-3 μm, and the weight ratio of the particle sizes of 1-2 μm and 2-3 μm is (60wt%-100wt%): (0wt%-40wt%).

3. The high temperature co-fired ceramic printing paste according to claim 1, characterized in that: The inorganic bonding phase comprises 95-99 wt % of powdered Al2O3 and 1-5 wt % of a sintering aid.

4. The high temperature co-fired ceramic printing paste according to claim 3, characterized in that: The sintering aid comprises: 1wt% to 3wt% of SiO2 and 1wt% to 2wt% of CaCO3.

5. The high temperature co-fired ceramic printing paste according to claim 1, characterized in that: The organic vehicle comprises 5 to 15 wt % of a thickener and 85 to 95 wt % of a solvent.

6. The high temperature co-fired ceramic printing paste according to claim 5, characterized in that: The thickener is any one of methyl cellulose, ethyl cellulose, polyvinyl alcohol, polyvinyl butyrate, polyvinyl acid, phenolic resin and epoxy resin, or a mixture of two or more thereof.

7. The high temperature co-fired ceramic printing paste according to claim 5, characterized in that: The solvent is any one of methanol, ethanol, toluene, acetone, xylene, butyl acetate, terpineol and butyl carbitol, or a mixture of two or more thereof.

8. A method for preparing a high temperature co-fired ceramic printing paste, characterized in that: The method comprises the following steps: Preparation of metallized powder: a certain number of ball milling beads are placed in a ball milling jar, and then tungsten powder and inorganic binder phase are placed in the ball milling jar for dry grinding. After the ball milling is completed, the ball milling beads and metallized powder are separated to obtain a mixture of tungsten powder and inorganic phase powder; Preparation of organic carrier: Heat the solvent in the organic carrier in a water bath at 60-80°C, then add the thickener while stirring until the thickener is completely dissolved; The preparation steps of the metallized tungsten slurry are as follows: tungsten powder, a mixture of inorganic phase powder and an organic carrier are mixed and placed in a homogenizer for stirring to obtain a mixed tungsten slurry, and the quickly stirred mixed slurry is ground multiple times with a three-roll mill to obtain the required metallized tungsten slurry for multi-layer alumina ceramics.

9. The method for preparing a high temperature co-fired ceramic printing paste according to claim 8, characterized in that: The ball milling time of the tungsten powder and the inorganic binder phase is 24 to 48 hours. After the ball milling is completed, the ball milling beads and the metallized powder are separated by a 300-mesh sieve.

10. The method for preparing a high temperature co-fired ceramic printing paste according to claim 8, characterized in that: The stirring speed in the homogenizer is 1000-2000 rpm.

Citation Information

Patent Citations

  • Alumina multilayer ceramic tungsten metallide slurry and preparation method thereof

    CN105060940A

  • High-temperature co-fired ceramic thick-film conductor paste

    CN107464600A

  • Tungsten slurry for printing white aluminum oxide multilayer ceramic substrate and preparation method of tungsten slurry

    CN112951477A

  • Pore-filling slurry for high-temperature co-fired ceramic

    CN113620718A

  • Multi-layer aluminum oxide ceramic metallized tungsten slurry for HTCC and preparation method of multi-layer aluminum oxide ceramic metallized tungsten slurry

    CN114380624A