Polyurethane coating material and coated fertilizer
By using polyurethane envelope materials with polyols, isocyanate components and other additives, the problem of poor film formation effect of polyurethane envelope materials is solved, forming a dense film, extending the release time of fertilizer, and improving fertilizer utilization and crop yield , reducing resource waste and environmental pollution.
Patent Information
- Application Number
- CN202411091725.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
AI Technical Summary
The existing polyurethane envelope materials have poor film formation effect and unstable chemical properties, which leads to inconsistent fertilizer release time and crop nutrient absorption, reduce fertilizer utilization, and cause resource waste and economic losses.
Polyurethane envelope materials using polyols, isocyanate components, 1,4-butanediol, synergists and lubricants are used to form dense films through specific mass ratios and preparation methods, thereby improving film formation effect and chemical stability. And mix the fertilizer with polyurethane envelope material to prepare polyurethane envelope fertilizer.
It improves the energy efficiency during the coating process, enhances the compressive resistance, extends the nutrient release time, improves fertilizer utilization, reduces nutrient loss and environmental pollution, and realizes one-time fertilization, which has significant ecological and economic benefits.
Smart Images

Figure CN118930360A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of controlled-release fertilizer preparation technology, specifically to a polyurethane coating material and a coated fertilizer. Background Technology
[0002] Coating materials are a class of materials used to cover or encapsulate other substances. They protect the encapsulated substance or control the release rate of the substance by forming a thin film. Coating materials are widely used in many fields, including plastic packaging films, mobile phone screen protectors, and fertilizer coatings.
[0003] The most widely used application is fertilizer coating. This type of fertilizer has a semi-permeable or insoluble film coated on the surface of water-soluble fertilizer particles. By controlling the release rate of nutrients, the fertilizer utilization rate is improved. It is mainly divided into slow-release fertilizer and controlled-release fertilizer.
[0004] Slow-release fertilizers transform into usable nutrients for plants more slowly after being applied to the soil than ordinary fertilizers. Their release rate, mode, and duration cannot be well controlled and are greatly affected by fertilization methods and environmental conditions. Controlled-release fertilizers, on the other hand, use certain measures to pre-set the fertilizer release time, synchronizing its nutrient release pattern with crop nutrient absorption, thereby improving fertilizer efficiency.
[0005] Polyurethane has become a commonly used coating material due to its advantages such as low temperature resistance, good flexibility, and good adhesion. However, existing polyurethane coating materials have poor film-forming effect and unstable chemical properties, often decomposing too early or too late. This leads to a mismatch between fertilizer release time and crop nutrient absorption time, reducing fertilizer utilization, wasting resources, seriously affecting crop growth, and resulting in economic losses.
[0006] Therefore, providing a polyurethane coating material with good film-forming effect and stable chemical properties, as well as a coated fertilizer, has become an urgent problem to be solved. Summary of the Invention
[0007] To address the problems of poor film-forming effect and unstable chemical properties of existing polyurethane coating materials, this invention provides a polyurethane coating material and a coated fertilizer.
[0008] The polyurethane coating material comprises polyol, isocyanate component, 1,4-butanediol, synergist and lubricant, in a mass ratio of (35-55):(40-52):(1.5-4.5):(0-0.5):(5-6.5).
[0009] Preferably, the synergist is triethylamine.
[0010] Preferably, the polyol is PEG2000;
[0011] Preferably, the isocyanate component comprises MDI-50 and castor oil in a mass ratio of (0.8-2.1):1.
[0012] The preparation method of the polyurethane-coated fertilizer is as follows: the fertilizer is mixed with a mass of polyurethane coating material A, heated and stirred, and then cooled to obtain polyurethane-coated fertilizer.
[0013] Preferably, after obtaining the polyurethane-coated fertilizer, it is preheated again, and then A quality of polyurethane coating material is added, and stirring is continued. After cooling, a multi-layer coated fertilizer is produced.
[0014] Preferably, the total mass A is 1-1.5% of the total mass of the fertilizer.
[0015] Preferably, the fertilizer is urea.
[0016] The present invention has the following advantages:
[0017] (1) The polyurethane coating material prepared by the present invention can reduce energy loss during the coating process, enhance the compressive strength of the coated fertilizer, and form a relatively dense film to prolong the nutrient release time.
[0018] (2) The polyurethane-coated fertilizer provided by the present invention can achieve reasonable fertilizer input without increasing fertilizer cost, while improving fertilizer utilization, reducing nutrient loss, reducing environmental pollution, and achieving one-time fertilization. It directly solves the impact of the shortage of rural labor on agricultural production and has obvious ecological and economic benefits. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0020] Figure 1 The following are the effect graphs of each control group in Experiment 1.
[0021] Figure 2 The images show the results of each experimental group in Experiment Example 2.
[0022] Figure 3 The nutrient release characteristic curve of polyurethane-coated urea.
[0023] Figure 4 Wheat yield for different treatments. Detailed Implementation
[0024] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0025] Experimental Example 1
[0026] Five control groups were set up in this experiment. Coating materials were prepared using different proportions of polymeric MDI (diphenylmethane diisocyanate), paraffin, PEG2000, castor oil, 1,4-butanediol, triethylamine and chitosan. The proportions of each component are shown in Table 1.
[0027] The preparation steps are as follows: At 75°C, polymeric MDI and paraffin were mixed to obtain component A; at 75°C, PEG2000, castor oil, 1,4-butanediol, triethylamine, and chitosan were mixed to obtain component B; in a petri dish, component A and component B were mixed and heated at 75°C for 10 minutes, then removed and cooled to room temperature to obtain the coating material. The results are shown in the appendix. Figure 1 .
[0028] Table 1
[0029]
[0030] Combine Table 1 and Appendix Figure 1 It can be seen that the coating materials prepared in control groups 1-5 all had poor film-forming properties, therefore polymeric MDI is not suitable for the preparation of coating materials.
[0031] Experimental Example 2
[0032] This experiment set up 10 experimental groups to prepare coating materials using different proportions of MDI-50 (diphenylmethane diisocyanate), paraffin, PEG2000, castor oil, 1,4-butanediol and triethylamine. The proportions of each component are shown in Table 2.
[0033] The preparation steps are as follows:
[0034] In experimental groups 1-6, MDI-50 and paraffin were mixed at 75℃ to obtain component A; PEG2000, castor oil, 1,4-butanediol, and triethylamine were mixed evenly at 75℃ to obtain component B; components A and B were mixed in a petri dish, heated at 75℃ for 10 minutes, removed, and cooled to room temperature to obtain the coating material. The results are shown in the appendix. Figure 2 .
[0035] In experimental groups 7-10, MDI-50, paraffin wax, PEG2000, castor oil, 1,4-butanediol, and triethylamine were mixed in a test tube. After 30 seconds, the mixture was poured into a petri dish and heated at 75°C for 10 minutes. The mixture was then removed and cooled to room temperature to obtain the coating material. The results are shown in the appendix. Figure 2 .
[0036] The polyurethane coating material comprises polyol, isocyanate component, 1,4-butanediol, synergist and lubricant, in a mass ratio of (35-55):(40-52):(1.5-4.5):(0-0.5):(5-6.5);
[0037] Table 2
[0038]
[0039] Combined with appendix Figure 2 As shown in Table 2, experimental groups 1 and 2 failed to form films after several hours of standing due to the absence of a chain extender (1,4-butanediol), and experimental group 6 also showed poor film formation. Experiments 3-5 and 7-9, after adding the chain extender (1,4-butanediol), yielded uniform membrane materials. Experiments 1-10 demonstrate that the addition of triethylamine promotes membrane formation, and the entire reaction process is very mild, with no bubble generation, making it suitable for the development of polyurethane-coated urea.
[0040] Experimental Example 3
[0041] Urea granules were loaded into a rotating drum and preheated to a set temperature of 75°C. Then, MDI-50, PEG2000, castor oil, 1,4-butanediol, triethylamine, and paraffin were added to the drum in a mass ratio of 35:57:3.0:0.6:4.4. The mixture was stirred at 11 r / min until homogeneous, allowing the materials to disperse evenly and gradually cross-link and solidify, forming the first coating. After the urea granules regained their fluidity, the same mass of MDI-50, PEG2000, castor oil, 1,4-butanediol, triethylamine, and paraffin were added to form the second coating. The third coating was obtained in the same manner as the second coating. After natural cooling, polyurethane-coated urea was obtained. The total mass of the polyol component, isocyanate component, and paraffin was 1% of the total mass of the urea.
[0042] According to the "Rapid Detection Method for Nutrient Release Period and Release Rate of Slow-Release and Controlled-Release Fertilizers" (HG / T4216-2011), extraction was performed at 25℃. 12.50g of undiluted coated urea sample was placed in a 150μm (100 mesh) finger-shaped nylon mesh bag (mesh bag specifications: 2-3cm wide, 15-20cm long, with a sealing rope and label attached). The bag was then placed in a culture flask containing 250ml of deionized water at a fertilizer-to-water ratio of 1:20 and incubated statically in a 25℃ biochemical constant temperature incubator. Sampling and measurements were performed periodically (see HG / T 4216-2011 for details). Results are attached. Figure 3 .
[0043] Test Example 4
[0044] The experiment was conducted from October 8, 2022 to June 15, 2023 at the experimental base of the Dezhou Academy of Agricultural Sciences in Huangheya Town, Dezhou. Two treatments were established: T1: conventional fertilization (FP), i.e., application of ordinary urea; T2: controlled-release fertilizer treatment (CRF), i.e., application of prepared polyurethane-coated urea. Each treatment was designed as a large-area experiment with an area of 270 m². 2 The tested soil was alluvial soil, and its physicochemical properties were as follows: total nitrogen 0.80 g / kg, available nitrogen 26.56 mg / kg, available phosphorus 34.27 mg / kg, available potassium 117.00 mg / kg, organic matter 13.17 g / kg, pH 8.59. The wheat variety used was Shannong 21.
[0045] The amount of fertilizer applied is shown in Table 1. The phosphate fertilizer is superphosphate (43%), the potassium fertilizer is potassium sulfate (50%), and the nitrogen fertilizer is urea. The basal application and top dressing are applied by broadcasting.
[0046] Table 1
[0047]
[0048] As shown in Table 1, the amount of nitrogen fertilizer used in the controlled-release nitrogen fertilizer treatment (CRF) was reduced by 45 kg / hm compared to the farmer's usual practice (FP). 2 The amount decreased by 14.3%.
[0049] 5m samples were taken at the wheat maturity stage. 2 Wheat yield was measured using quadrats to calculate the wheat yield per unit area. The wheat yield results are shown below. Figure 2 The controlled-release urea treatment resulted in a wheat yield of 10204.2 kg / hm². 2 The yield per hectare is higher than the 9724.4 kg / hm² that farmers are accustomed to. 2 It was 480.1 kg higher, with a yield increase of 5%.
[0050] The coated urea made using the coating material of this invention can increase wheat yield by 5% compared to farmers' usual practice while reducing nitrogen fertilizer usage by 14.3%, showing promising application prospects.
[0051] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A polyurethane coating material, characterized in that: The invention comprises polyol, isocyanate component, 1,4-butanediol, synergist and lubricant, and the mass ratio is (35-55):(40-52):(1.5-4.5):(0-0.5):(5-6.5).
2. A polyurethane coating material according to claim 1, characterized in that: The synergist is triethylamine.
3. A polyurethane coating material according to claim 1, characterized in that: The polyol is PEG2000.
4. The polyurethane coating material according to claim 1, characterized in that: The isocyanate component includes MDI-50 and castor oil in a mass ratio of (0.8-2.1):
1.
5. The polyurethane coating material according to claim 1, characterized in that: The lubricant is paraffin.
6. Use of the polyurethane coating material according to any one of claims 1 to 5, characterized in that: Used to prepare polyurethane coated fertilizers.
7. The use of the polyurethane coating material according to claim 6, characterized in that: The preparation method of the polyurethane coated fertilizer comprises the following steps: mixing the fertilizer with a polyurethane coating material of quality A, heating and stirring, and cooling to obtain the polyurethane coated fertilizer.
8. The method for preparing a polyurethane coated fertilizer according to claim 7, characterized in that: After the polyurethane coated fertilizer is obtained, the polyurethane coating material of quality A is added, heated and stirred, and a multi-layer coated fertilizer is obtained after cooling.
9. The method for preparing a polyurethane coated fertilizer according to claim 7, characterized in that: The mass of A is 1-1.5% of the total mass of the fertilizer.
10. The method for preparing a polyurethane coated fertilizer according to claim 7, characterized in that: The fertilizer is urea granules.