Coated urea as well as production method and application thereof

By wrapping the hydrogel film on the surface of the urea, combining zeolite powder and toughener, the compatibility problem caused by urea hygroscopicity is solved, the compatibility and stability of urea and organic fertilizer are achieved, and the application effect of base fertilizer is improved.

CN118930364APending Publication Date: 2024-11-12河北萌帮生物科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411131338.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-17
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Urea has strong hygroscopicity, which makes it impossible to mix with humic acid large-grain organic fertilizer as a base fertilizer.

Method used

Using the technology of enveloped urea, a layer of hydrogel-type film is wrapped on the surface of the urea, and a three-dimensional spatial structure is formed using borax, polyvinyl alcohol and functional additives to prevent the urea from hygroscopicity, and the structure is improved through zeolite powder and toughener. Stability to ensure compatibility between urea and organic fertilizer.

Benefits of technology

It effectively reduces the hygroscopicity of urea, so that it can be mixed with humic acid large-grain organic fertilizer, and used as base fertilizer, which improves the use value of urea and the utilization rate of organic fertilizer, while preventing deflated in transportation and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930364A_ABST
    Figure CN118930364A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of agriculture, and provides coated urea as well as a production method and application thereof. The coated urea is of a core-shell structure, an inner core of the core-shell structure is urea, a shell of the core-shell structure is an adhesive film, and raw materials of the adhesive film comprise a hydrogel body and a functional additive; the hydrogel body comprises borax, polyvinyl alcohol and a suspending agent; the functional auxiliary agent comprises a filling agent and a toughening agent. According to the technical scheme, the problem that urea in the prior art is high in hygroscopicity and cannot be mixed with a humic acid large-particle organic fertilizer to serve as a base fertilizer is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of agricultural technology, and in particular to coated urea and a production method and application thereof. Background Art

[0002] Urea is a neutral fertilizer that is easy to use and has little destructive effect on the soil. It is a chemical nitrogen fertilizer with a large usage amount and the highest nitrogen content. It is suitable for various soils and plants. However, it has strong hygroscopicity and is easy to clump after absorbing moisture. It is not suitable for storage in a humid environment.

[0003] Humic acid large-particle organic fertilizer is obtained by disc granulation from fermented lignite. It has the function of improving soil structure and increasing soil fertility. When mixed with urea and used as base fertilizer, it has a good promoting effect on the growth of crops. However, due to the preparation process of humic acid large-particle organic fertilizer and the properties of fermented lignite itself, the moisture content of the system is 20%~30%. When urea and the organic fertilizer are mixed, as time goes by, urea will absorb the moisture in the organic fertilizer, causing the urea to dissolve. Therefore, after the two are mixed, they cannot be used as base fertilizer. Summary of the invention

[0004] The present invention provides coated urea and a production method and application thereof, which solve the problem in the related art that urea has strong hygroscopicity and cannot be mixed with humic acid large-particle organic fertilizer for use as base fertilizer.

[0005] The technical solution of the present invention is as follows: A coated urea is a core-shell structure, wherein the core of the core-shell structure is urea and the shell is a film, and the raw materials of the film include a hydrogel body and a functional additive; The hydrogel body comprises borax, polyvinyl alcohol and a suspending agent; The functional additives include fillers and toughening agents.

[0006] As a further technical solution, the functional auxiliary agent also includes a preservative, and the mass ratio of the hydrogel body to the functional auxiliary agent is 8~12:23~38.

[0007] As a further technical solution, the filler includes one or both of zeolite powder and talc; the preservative includes one or more of sodium benzoate, kasone, and potassium sorbate; and the toughening agent includes one or both of calcium carbonate and titanium dioxide.

[0008] As a further technical solution, the particle size of the urea is 1.5~5mm.

[0009] As a further technical solution, the suspending agent includes one or more of xanthan gum, sodium alginate, and sodium carboxymethyl cellulose.

[0010] As a further technical solution, the mass ratio of the borax, polyvinyl alcohol and suspending agent is 4-5:3-5:1-2; the mass ratio of the urea to polyvinyl alcohol is 1000:3-5.

[0011] The invention limits the mass ratio of borax, polyvinyl alcohol and suspending agent to 4-5:3-5:1-2, thereby further reducing the hygroscopicity of urea.

[0012] As a further technical solution, the mass ratio of the filler, preservative and toughening agent is 20~30:1~3:2~5.

[0013] The present invention also proposes a method for producing coated urea, comprising the following steps: S1. After mixing polyvinyl alcohol with water, add 1 / 2 to 1 / 3 of the mass of suspending agent and filler to obtain solvent A; S2, after mixing borax with water, add the remaining suspending agent and the remaining functional additives to obtain solvent B; S3. Spraying solvent A and solvent B on the surface of urea in sequence to obtain coated urea.

[0014] The present invention suspends water-insoluble zeolite powder in a polyvinyl alcohol solution. When the borax solution and the polyvinyl alcohol solution are mixed to form a three-dimensional space structure, the zeolite powder will automatically fill the space structure, and then the water is dried at a suitable temperature to form a stable protective shell on the surface of urea. At the same time, by adding a proper amount of toughening agent, the stability and strength of the zeolite powder are improved, the hygroscopicity of urea is better prevented, and it is ensured that the coated urea can be mixed with organic fertilizer, and there will be no powder shedding during transportation and handling.

[0015] In the present invention, solvent A is equivalent to a thickener, so solvent A is sprayed first to wet the entire surface of urea; and solvent B is a cross-linking agent, which can cross-link with solvent A to form a gel. If solvent B is sprayed first, the wetted urea will be uneven, thereby reducing the various properties of the coated urea. Therefore, the present invention further reduces the hygroscopicity of urea by limiting the production method of coated urea.

[0016] As a further technical solution, the mass ratio of the polyvinyl alcohol to water is 3-5:100; the mass ratio of borax to water is 4-5:100.

[0017] As a further technical solution, the spraying process is carried out in a round pan granulator.

[0018] As a further technical solution, the spraying process is accompanied by drying, the drying temperature is 70-80° C., and the drying time is 20-30 minutes.

[0019] As a further technical solution, the spraying process is accompanied by stirring, and the stirring speed is 100-200 rpm.

[0020] The invention also proposes the application of the coated urea or the coated urea produced by the production method in base fertilizer.

[0021] The working principle and beneficial effects of the present invention are: 1. The present invention provides a coated urea, which prevents the moisture absorption of urea by coating a layer of hydrogel film on the surface of urea, does not affect the release of urea in the soil, increases the slow-release performance of urea, and improves the use value of urea. In addition, after mixing the humic acid large-particle organic fertilizer with the coated urea of ​​the present invention, it can be used as a base fertilizer.

[0022] 2. The coated urea in the present invention is a core-shell structure, wherein the shell is a film, and the raw materials of the film include a hydrogel body and a functional additive. The hydrogel body is formed by mixing a borax solution and a polyvinyl alcohol solution to form a three-dimensional hydrogel spatial network structure, and then by adding a functional additive in the spatial network structure, it is wrapped on urea through processing, thereby blocking the hygroscopic property of urea, so that urea can be mixed with humic acid particles, and applied to crops as a base fertilizer, thereby improving the utilization rate of humic acid organic fertilizer. In addition, the addition of zeolite powder in the three-dimensional spatial network structure plays a role in preventing the hygroscopic effect of urea, but the structural strength of the zeolite powder is small, non-viscous, and may fall off with the friction between urea. The network structure of the hydrogel makes its structure stable, and the hardness is increased by adding a tough additive.

[0023] 3. The present invention uses polyvinyl alcohol (PVA) as a thickener and borax (Na2B4O7•10H2O, Borax) as a crosslinking agent. Polyvinyl alcohol and borax are physically crosslinked, and have the characteristics of easy decomposition and high stability. The borate bond is the physical crosslinking point. Borax-PVA hydrogel is obtained by simple physical mixing. First, polyvinyl alcohol is dissolved in water to form a uniform solution, and the borate ion B(OH)4 − It cross-links with the hydroxyl groups of polyvinyl alcohol to form a hydrogel, which in turn forms an ordered three-dimensional network space structure with pores and morphological structures, providing storage space for zeolite powder, which can better evenly wrap the zeolite powder on urea and prevent powdering. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0025] Figure 1 Schematic diagram of borate ester bond formed after mixing polyvinyl alcohol (PVA) solution and borax (Na2B4O7•10H2O) solution; Figure 2This is the infrared spectrum of the borate ester bond formed after cross-linking of polyvinyl alcohol (PVA) solution and borax (Na2B4O7•10H2O) solution. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] The parameters of the raw materials in the following examples and comparative examples are as follows: Urea has a nitrogen content of 46.44%, white particles with a particle size of 2~4mm; The weight average molecular weight of polyvinyl alcohol is 70,000-80,000, and the alcoholysis degree is 98%-99%; Borax (Na2B4O7•10H2O): content ≥99.5%; Zeolite powder: 1200 mesh; Talc: 1200 mesh; Xanthan gum: food grade, content ≥99.9%; Sodium alginate: food grade, content ≥99.9%; Sodium carboxymethyl cellulose: content ≥98%; Sodium benzoate: content ≥99.5%; Kason: Model XS-602, purchased from Hebei Xingshan Environmental Protection Technology Co., Ltd.; Calcium carbonate: powder, content ≥98%, purchased from Tianjin Shentai Chemical Reagent Co., Ltd.; Titanium dioxide: powder, content ≥99%, purchased from Tianjin Shentai Chemical Reagent Co., Ltd.

[0028] Example 1 (1) Mix 3 g of polyvinyl alcohol with 97 g of water, stir at 90 °C for 45 min to dissolve, cool to room temperature, add 0.5 g of xanthan gum and 20 g of zeolite powder, and mechanically stir for 1 h as solvent A; (2) Dissolve 4 g of borax in 96 g of water, add 0.5 g of xanthan gum, 1 g of sodium benzoate, and 2 g of calcium carbonate, and stir mechanically for 1 h as solvent B; (3) Place 1000 g of urea in a round pot, adjust the rotation speed to 100 rpm, and dry at 70 °C. First spray 30 g of solvent A, then spray 5 g of solvent B after a 2-min interval. Continue drying for 20 min to obtain coated urea.

[0029] Example 2 (1) Mix 4 g of polyvinyl alcohol with 96 g of water, stir at 90 °C for 45 min to dissolve, cool to room temperature, add 0.8 g of sodium alginate and 30 g of talc, and stir mechanically for 1 h as solvent A; (2) Dissolve 5 g of borax in 95 g of water, add 0.8 g of sodium alginate, 2 g of kason, and 3 g of titanium dioxide, and stir mechanically for 1 h as solvent B; (3) Place 1000 g of urea in a round pot, adjust the rotation speed to 200 rpm, and dry at 80 °C. First spray 30 g of solvent A. After a 2-min interval, spray 5 g of solvent B. Continue drying for 30 min to obtain coated urea.

[0030] Example 3 (1) Mix 5 g of polyvinyl alcohol with 95 g of water, stir at 90 °C for 45 min to dissolve, cool to room temperature, add 1 g of sodium carboxymethyl cellulose and 20 g of zeolite powder, and stir mechanically for 1 h as solvent A; (2) Dissolve 4 g of borax in 96 g of water, add 1 g of sodium carboxymethyl cellulose, 3 g of potassium sorbate, and 4 g of calcium carbonate, and stir mechanically for 1 h as solvent B; (3) Place 1000 g of urea in a round pot, adjust the rotation speed to 100 rpm, and dry at 70 °C. First spray 30 g of solvent A. After a 2-min interval, spray 5 g of solvent B. Continue drying for 20 min to obtain coated urea.

[0031] Example 4 (1) Mix 3 g of polyvinyl alcohol with 97 g of water, stir at 90 °C for 45 min to dissolve, cool to room temperature, add 0.5 g of xanthan gum and 30 g of talcum powder, and stir mechanically for 1 h as solvent A; (2) Dissolve 4 g of borax in 96 g of water, add 1 g of xanthan gum, 2 g of sodium benzoate, and 5 g of titanium dioxide, and stir mechanically for 1 h as solvent B; (3) Place 1000 g of urea in a round pot, adjust the rotation speed to 100 rpm, and dry at 80 °C. First spray 30 g of solvent A. After a 2-min interval, spray 5 g of solvent B. Continue drying for 20 min to obtain coated urea.

[0032] Example 5 (1) Mix 4 g of polyvinyl alcohol with 96 g of water, stir at 90 °C for 45 min to dissolve, cool to room temperature, add 0.5 g of sodium carboxymethyl cellulose and 30 g of zeolite powder, and stir mechanically for 1 h as solvent; (2) Dissolve 4 g of borax in 96 g of water, add 0.5 g of sodium carboxymethyl cellulose, 3 g of sodium benzoate, and 4 g of calcium carbonate, and stir mechanically for 1 h as solvent B; (3) Place 1000 g of urea in a round pot, adjust the rotation speed to 100 rpm, and dry at 70 °C. First spray 30 g of solvent A. After a 2-min interval, spray 5 g of solvent B. Continue drying for 30 min to obtain coated urea.

[0033] Example 6 (1) Mix 5 g of polyvinyl alcohol with 95 g of water, stir at 90 °C for 45 min to dissolve, cool to room temperature, add 1 g of sodium alginate and 30 g of talc, and stir mechanically for 1 h as solvent A; (2) Dissolve 5 g of borax in 95 g of water, add 1 g of sodium alginate, 3 g of kason, and 5 g of titanium dioxide, and stir mechanically for 1 h as solvent B; (3) Place 1000 g of urea in a round pot, adjust the rotation speed to 200 rpm, and dry at 80 °C. First spray 30 g of solvent A. After a 2-min interval, spray 5 g of solvent B. Continue drying for 20 min to obtain coated urea.

[0034] Example 7 (1) Mix 3 g of polyvinyl alcohol with 97 g of water, stir at 90 °C for 45 min to dissolve, cool to room temperature, add 0.5 g of xanthan gum and 20 g of zeolite powder, and mechanically stir for 1 h as solvent A; (2) Dissolve 1 g of borax in 96 g of water, add 0.5 g of xanthan gum, 1 g of sodium benzoate, and 2 g of calcium carbonate, and stir mechanically for 1 h as solvent B; (3) Place 1000 g of urea in a round pot, adjust the rotation speed to 100 rpm, and dry at 70 °C. First spray 30 g of solvent A. After a 2-min interval, spray 5 g of solvent B. Continue drying for 20 min to obtain coated urea.

[0035] Example 8 (1) Mix 3 g of polyvinyl alcohol with 97 g of water, stir at 90 °C for 45 min to dissolve, cool to room temperature, add 0.5 g of xanthan gum and 20 g of zeolite powder, and mechanically stir for 1 h as solvent A; (2) Dissolve 8 g of borax in 96 g of water, add 0.5 g of xanthan gum, 1 g of sodium benzoate, and 2 g of calcium carbonate, and stir mechanically for 1 h as solvent B; (3) Place 1000 g of urea in a round pot, adjust the rotation speed to 100 rpm, and dry at 70 °C. First spray 30 g of solvent A. After a 2-min interval, spray 5 g of solvent B. Continue drying for 20 min to obtain coated urea.

[0036] Example 9 (1) Mix 3 g of polyvinyl alcohol with 97 g of water, stir at 90 °C for 45 min to dissolve, cool to room temperature, add 0.5 g of xanthan gum and 20 g of zeolite powder, and mechanically stir for 1 h as solvent A; (2) Dissolve 4 g of borax in 96 g of water, add 0.5 g of xanthan gum, 1 g of sodium benzoate, and 2 g of calcium carbonate, and stir mechanically for 1 h as solvent B; (3) Put 1000g of urea into a round pot, adjust the speed to 100rpm, and dry at 70℃. First spray 5g of solvent B, then spray 30g of solvent A after 2 minutes, and continue drying for 20 minutes to obtain coated urea.

[0037] Comparative Example 1 (1) Mix 3 g of polyvinyl alcohol with 97 g of water, stir at 90 °C for 45 min to dissolve, cool to room temperature, add 0.5 g of xanthan gum, and mechanically stir for 1 h as solvent A; (2) Dissolve 4 g of borax in 96 g of water, add 0.5 g of xanthan gum and 1 g of sodium benzoate, and stir mechanically for 1 h as solvent B; (3) Place 1000 g of urea in a round pot, adjust the rotation speed to 100 rpm, and dry at 70 °C. First spray 30 g of solvent A. After a 2-min interval, spray 5 g of solvent B. Continue drying for 20 min to obtain coated urea.

[0038] Comparative Example 2 (1) Mix 3 g of polyvinyl alcohol with 97 g of water, stir at 90 °C for 45 min to dissolve, cool to room temperature, add 0.5 g of xanthan gum, and mechanically stir for 1 h as solvent A; (2) Dissolve 4 g of borax in 96 g of water, add 0.5 g of xanthan gum, 1 g of sodium benzoate, and 2 g of calcium carbonate, and stir mechanically for 1 h as solvent B; (3) Place 1000 g of urea in a round pot, adjust the rotation speed to 100 rpm, and dry at 70 °C. First spray 30 g of solvent A. After a 2-min interval, spray 5 g of solvent B. Continue drying for 20 min to obtain coated urea.

[0039] Comparative Example 3 (1) Mix 3 g of polyvinyl alcohol with 97 g of water, stir at 90 °C for 45 min to dissolve, cool to room temperature, add 0.5 g of xanthan gum and 20 g of zeolite powder, and mechanically stir for 1 h as solvent A; (2) Dissolve 4 g of borax in 96 g of water, add 0.5 g of xanthan gum and 1 g of sodium benzoate, and stir mechanically for 1 h as solvent B; (3) Place 1000 g of urea in a round pot, adjust the rotation speed to 100 rpm, and dry at 70 °C. First spray 30 g of solvent A. After a 2-min interval, spray 5 g of solvent B. Continue drying for 20 min to obtain coated urea.

[0040] Comparative Example 4 (1) Add 0.5 g xanthan gum and 20 g zeolite powder to 97 g water and stir mechanically for 1 h as solvent A; (2) Add 0.5 g xanthan gum, 1 g sodium benzoate, and 2 g calcium carbonate to 96 g water and stir mechanically for 1 hour as solvent B; (3) Place 1000 g of urea in a round pot, adjust the rotation speed to 100 rpm, and dry at 70 °C. First spray 30 g of solvent A, then spray 5 g of solvent B after a 2-min interval. Continue drying for 20 min to obtain coated urea.

[0041] The hardness of 30 coated ureas obtained in Examples 1 to 9 and Comparative Examples 1 to 4 was measured at random, and the average value was taken; then, the coated ureas were placed at a humidity of 60% and a temperature of 45° C. for 20 days, and 30 coated ureas were measured at random again, and the average value was taken. The difference between the two was used to characterize the hygroscopicity. The results are recorded in Table 1.

[0042] Table 1 Hardness of coated urea

[0043] As can be seen from Table 1, the hardness of the coated urea obtained in Examples 1 to 9 did not decrease significantly after being placed for 20 days, indicating that the hygroscopicity was small, while the coated urea without zeolite powder and toughening agent in Comparative Example 1 dissolved, and the coated urea without zeolite powder in Comparative Example 2 dissolved, indicating that the zeolite powder played a role in blocking urea moisture absorption in the three-dimensional space structure; and the hardness of the coated urea without toughening agent in Comparative Example 3 decreased significantly, indicating that the toughening agent can increase the hardness of zeolite powder, making the zeolite powder more compact in three-dimensional space, and also affecting the hygroscopicity of the coated urea. In Comparative Example 4, the coated urea without polyvinyl alcohol and borax and with zeolite powder and toughening agent, although the hardness decreases not significantly, is easy to de-powder when mixed with humic acid large-particle organic fertilizer, indicating that the three-dimensional space structure formed by cross-linking polyvinyl alcohol and borax provides a stable storage space for zeolite powder and toughening agent.

[0044] Figure 1 Schematic diagram of the borate ester bond formed after mixing polyvinyl alcohol (PVA) solution and borax (Na2B4O7•10H2O) solution.

[0045] Figure 2 This is the infrared spectrum of the borate ester bond formed after cross-linking of polyvinyl alcohol (PVA) solution and borax (Na2B4O7•10H2O) solution.

[0046] Depend on Figure 2 It can be seen that compared with the absorption peak of PVA, the hydrogel (i.e., the coated urea in Example 1) has an absorption peak at 1650 cm -1 There is an absorption peak of bending vibration (boric acid ester bond is a special double bond), indicating the formation of boric acid ester bond. PVA is at 3450cm -1 There is a broad absorption band at 3450 cm, which is caused by the stretching vibration of OH (polymer), while the hydrogel (i.e., the coated urea in Example 1) has a broad absorption band at 3450 cm -1 The broad peak at is reduced to a sharp peak. This is because borate bonds are formed between polyvinyl alcohol and borax, forming a cross-linked structure and reducing the amplitude of OH vibration.

[0047] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A coated urea having a core-shell structure, characterized in that: The core of the core-shell structure is urea, and the shell is a film, and the raw materials of the film include a hydrogel body and a functional additive; The hydrogel body comprises borax, polyvinyl alcohol and a suspending agent; The functional additives include fillers and toughening agents.

2. The coated urea according to claim 1, characterized in that: The functional additive also includes a preservative, and the mass ratio of the hydrogel body to the functional additive is 8-12:23-38.

3. A coated urea according to claim 2, characterized in that: The filler includes one or both of zeolite powder and talc powder; the preservative includes one or both of sodium benzoate, kasone and potassium sorbate; the toughening agent includes one or both of calcium carbonate and titanium dioxide.

4. The coated urea according to claim 1, characterized in that: The suspending agent includes one or more of xanthan gum, sodium alginate and sodium carboxymethyl cellulose.

5. The coated urea according to claim 1, characterized in that: The mass ratio of the borax, polyvinyl alcohol and suspending agent is 4-5:3-5:1-2; the mass ratio of the urea to polyvinyl alcohol is 1000:3-5.

6. The coated urea according to claim 2, characterized in that: The mass ratio of the filler, preservative and toughening agent is 20-30:1-3:2-5.

7. The method for producing coated urea according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. After mixing polyvinyl alcohol with water, add 1 / 2 to 1 / 3 of the mass of suspending agent and filler to obtain solvent A; S2, after mixing borax with water, add the remaining suspending agent and the remaining functional additives to obtain solvent B; S3. Spraying solvent A and solvent B on the surface of urea in sequence to obtain coated urea.

8. The method for producing coated urea according to claim 7, characterized in that: The spraying process is accompanied by drying, the drying temperature is 70-80° C., and the drying time is 20-30 minutes.

9. The method for producing coated urea according to claim 7, characterized in that: The spraying process is accompanied by stirring, and the stirring speed is 100-200 rpm.

10. Use of the coated urea according to any one of claims 1 to 6 or the coated urea produced by the production method according to any one of claims 7 to 9 in base fertilizer.