Rare earth ferrous cyanate / melamine-derived multi-metal composite nitrogen-doped carbon burning rate catalyst

The multi-metal composite aza carbon combustion speed catalyst prepared by combining rare earth ferrocyanate and melamine solves the problem of low combustion efficiency of solid propellants, achieves the improvement of efficient combustion performance, and meets the combustion needs of modern spacecraft.

CN118930389AActive Publication Date: 2024-11-12SHAANXI NORMAL UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411011170.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The combustion efficiency of existing solid propellants is low, making it difficult to meet the demand for efficient combustion performance of modern spacecraft.

Method used

The combination of rare earth ferrocyanate and melamine is used to prepare polymetal composite aza carbon material as a combustion speed catalyst by calcining under the protection of inert gas, and g-C3N4 is used as a support to form rare earth ferrocyanate/melamine-derived polymetals. Compound aza carbon combustion rate catalyst to enhance catalytic performance.

Benefits of technology

The combustion efficiency of solid propellants is significantly improved, and through the synergistic effect between polymetals and the action of g-C3N4 support, it has excellent catalytic effect on the thermal decomposition of ammonia calcium, improving combustion performance and thermal stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930389A_ABST
    Figure CN118930389A_ABST
Patent Text Reader

Abstract

The invention discloses a rare earth ferrocyanate / melamine-derived multi-metal composite nitrogen-doped carbon burning rate catalyst, which is prepared by the following steps: dropwise adding a saturated aqueous solution of a soluble salt of a rare earth metal into a Na4 [Fe (CN) 6] saturated aqueous solution, reacting, and then carrying out solid-liquid separation, washing and drying to obtain rare earth ferrocyanate, and then carrying out ball-milling mixing on the rare earth ferrocyanate and melamine, and calcining under the protection of inert gas to prepare the rare earth ferrocyanate-melamine composite material. The preparation process of the burning rate catalyst is simple, low in cost and free of pollution, melamine and rare earth ferrocyanate are evenly mixed through a ball milling method, then transition metal Fe and rare earth metal particles are evenly loaded on the nitrogen-doped carbon material (g-C3N4) through high-temperature thermal condensation, and the burning rate catalyst is obtained. And the combustion rate catalytic performance of the catalyst on AP thermal decomposition is improved through the synergistic effect of multiple metals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid propellants, and in particular relates to a multi-metal composite nitrogen-carbon combustion rate catalyst derived from rare earth ferrocyanate / melamine. Background Art

[0002] Solid propellants, as an important component of missile and rocket engines, often provide power for rockets and missiles to take off. Their composition and performance affect the speed and flight time of rockets. Today's commonly used solid propellants can be roughly divided into two categories according to composition and structure, namely double-base propellants and composite propellants. Double-base propellants can be divided into modified double-base propellants and unmodified double-base propellants. Solid propellants are mainly composed of adhesives, oxidants, plasticizers, curing agents, burning rate regulators and other components. Among them, burning rate regulators are often divided into burning rate catalysts and burning rate inhibitors according to their effects on the burning rate of solid propellants. In order to adjust the combustion performance of solid propellants and improve the burning rate, it is often achieved by adding burning rate catalysts. As one of the most important components of solid propellants, its method of action is often to participate in the reaction by chemical methods, so as to improve the combustion performance of the propellant and achieve the launch needs of different engines and different propellants, thereby meeting the use needs of modern spacecraft.

[0003] Ferrocyanate, also known as Prussian blue and its analogs, is a complex with adjustable composition and open framework, and has typical physical and chemical characteristics of large framework materials. Prussian blue analogs often replace the iron ions and ferrous ions in Prussian blue with other metals to obtain higher specific surface area, stability and chemical properties. In catalytic applications, since metal compounds derived from Prussian blue and its analogs also have excellent stability, selectivity and precursor morphology, as well as good electronic conductivity and sufficient catalytic active sites, such materials have become hot materials in various research fields.

[0004] Rare earth metals are a general term for 17 metal elements, which are composed of lanthanide elements, scandium and yttrium. Many researchers have tried various metal combinations to conduct experiments, and rare earth compounds have outstanding effects on the catalysis of double-base propellant combustion and reducing the infrared attenuation of fuel gas. In other fields, the composite system of rare earth and other transition elements also has excellent catalytic performance. Because their outer electron configurations are almost the same, the properties of rare earth elements are very similar. For a long time, the multi-faceted application of rare earth resources has become one of the research hotspots.

[0005] Graphitic carbon nitride, g-C3N4, is a special non-metallic semiconductor, an amorphous synthetic compound, mainly formed by stacking two-dimensional CN sheets. As the most stable phase among the five allotropes of C3N4, g-C3N4 is insoluble in acids, alkalis and general organic solvents, has good thermal stability and chemical stability, and has the following significant advantages as a burning rate catalyst: simple preparation process, easy operation, high cost-effectiveness, environmental protection, non-toxicity, high temperature resistance, etc., showing that this material has good application prospects. These advantages have made g-C3N4 widely concerned in various reaction catalysis fields for a long time.

[0006] With the continuous deepening of research, many types of composite burning rate catalysts have emerged in the field of solid propellants. Chi Huang et al. proposed a self-template strategy to design and synthesize cobalt-rich hollow spherical Prussian blue analogs through a self-assembly process. The spherical hollow structure can provide a large specific surface area and more active sites. The thermal catalytic performance under the AP system was studied, and the catalytic advantages and macroscopic kinetic behavior of the catalyst were tested (Zeyu Z, Chi H, et al. Hierarchical MOFs with Good Catalytic Properties and Structural Stability in Oxygen-Rich and High-Temperature Environments. Small, 2024, 2(19): 2309302). Zheng Jiahong et al. used high-temperature carbonization to prepare a series of Fe and Mn Prussian blue analogs composite nitrogen-doped carbon nanosheet catalysts for the removal of Rhodamine B. The study showed that Prussian blue analogs were converted into nitrogen-doped carbon materials with high specific surface area, high porosity and high nitrogen content through high-temperature calcination or inert gas carbonization, which is of great significance for improving the catalytic performance of the catalyst (Zheng Jiahong, Zheng Xin. Preparation and activation of FeMnO derived from Fe-Mn Prussian blue analogs supported on nitrogen-doped graphitic carbon for the removal of Rhodamine B by monopersulfate. Journal of the Chinese Ceramic Society, 51(12):1-11). Danna Ma et al. reviewed the structure, properties, preparation and application of a series of g-C3N4 derivatives in catalytic AP thermal decomposition, and discussed in detail the enhanced catalytic mechanism of AP thermal decomposition (DN Ma, XQ Wang, et al. Research Development on Graphitic Carbon Nitride and Enhanced Catalytic Activity on Ammonium Perchlorate. RSC Adv., 2021, 11(10): 5729-5740).

[0007] In summary, in order to improve the combustion efficiency of propellants, adding a burning rate catalyst, an important component of propellants, is one of the reasonable and efficient methods. According to previous studies, carbon materials have been proved to be an excellent burning rate catalyst carrier, and ferrocyanate, namely Prussian blue and its analogs, is a complex with an adjustable framework, which has good stability and selectivity. It can form a metal-embedded nitrogen-carbon material through carbon condensation under high-temperature calcination. Therefore, combining rare earth ferrocyanate with g-C3N4 to prepare a new composite burning rate catalyst is one of the potential development directions in the field of catalytic materials. Summary of the invention

[0008] The purpose of the present invention is to provide a rare earth ferrocyanate / melamine derived multi-metal composite nitrogen-carbon combustion rate catalyst which is environmentally friendly, convenient and fast and has good catalytic performance.

[0009] In order to achieve the above-mentioned purpose, the rare earth ferrocyanate / melamine-derived multi-metal composite nitrogen-carbon combustion rate catalyst provided by the present invention is a multi-metal composite nitrogen-carbon material with g-C3N4 as a carrier to load Fe and rare earth metal particles, which is obtained by ball-milling rare earth ferrocyanate and melamine and then calcining under the protection of inert gas; wherein the rare earth ferrocyanate is selected from any one of Sm4[Fe(CN)6]3, Eu4[Fe(CN)6]3, Tb4[Fe(CN)6]3, and Dy4[Fe(CN)6]3; the mass ratio of the rare earth ferrocyanate to melamine is 1:1~4, and preferably the mass ratio of the rare earth ferrocyanate to melamine is 1:1.5~2.

[0010] The preparation method of the above-mentioned rare earth ferrocyanate is: a saturated aqueous solution of a soluble salt of a rare earth metal is added dropwise to a saturated aqueous solution of Na4[Fe(CN)6], and after reacting at room temperature for 1.5 to 4 hours, the obtained suspension is subjected to solid-liquid separation, and the solid is washed and dried to obtain rare earth ferrocyanate; wherein the soluble salt of the rare earth metal is selected from any one of Sm(NO3)3·6H2O, Eu(NO3)3·6H2O, Tb(NO3)3·6H2O, and Dy(NO3)3·6H2O; and the molar ratio of the rare earth metal elements in the soluble salt of the rare earth metal is 1 to 2:1.

[0011] Furthermore, the frequency of the ball mill is 25-50 Hz, the forward rotation time of the ball mill is 5-30 min, the interval time is 5 min, the reverse time is 5-30 min, and the cycle is repeated three times. Preferably, the frequency of the ball mill is 35-40 Hz, the forward rotation time of the ball mill is 10-15 min, the interval time is 5 min, the reverse time is 10-15 min, and the cycle is repeated three times.

[0012] Furthermore, the calcination temperature is 300-800°C, the holding time is 1-8h, and the heating rate is 1-10°C / min. Preferably, the calcination temperature is 450-550°C, the holding time is 4-6h, and the heating rate is 5-6°C / min.

[0013] Furthermore, the above-mentioned inert gas is argon.

[0014] The beneficial effects of the present invention are as follows:

[0015] The present invention mixes rare earth ferrocyanate and melamine in a certain ratio, calcines them under a certain calcination process, and introduces g-C3N4 prepared by high-temperature calcination of melamine to form a rare earth ferrocyanate / melamine derived multi-metal composite nitrogen-carbon material combustion rate catalyst. The composite combustion rate catalyst of the present invention has excellent performance and is environmentally friendly. On the one hand, it plays the role of a carrier of the g-C3N4 two-dimensional carbon material, and on the other hand, through the synergistic effect between multiple metals, it can have an excellent catalytic effect on the thermal decomposition of AP. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a scanning electron microscope image of the burning rate catalyst prepared in Example 1.

[0017] Figure 2 It is the differential scanning calorimetry curve of adding 5 wt.% of the burning rate catalyst prepared in Examples 1 to 4 into AP and pure AP.

[0018] Figure 3 It is the differential scanning calorimetry curve of AP with 5 wt.% of the burning rate catalyst prepared in Comparative Examples 1 to 5 added, AP with 5 wt.% of g-C3N4 added, and pure AP. DETAILED DESCRIPTION

[0019] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited to these embodiments.

[0020] Example 1

[0021] 90.6 mg (0.02 mmol) of Tb(NO3)3·6H2O was added to 30 mL of water to obtain a saturated aqueous solution of Tb(NO3)3; 96.8 mg (0.02 mmol) of Na4[Fe(CN)6]·10H2O was added to 20 mL of water to obtain a saturated aqueous solution of Na4[Fe(CN)6]; then the saturated aqueous solution of Tb(NO3)3 was added dropwise to the saturated aqueous solution of Na4[Fe(CN)6] using a dropper, and the reaction was stirred at 350 rpm for 2 h at room temperature to obtain a light green suspension; the centrifuge speed was set to The suspension was adjusted to 10000 rpm and the centrifugal time was 3 min to separate the solid and liquid, and washed repeatedly with deionized water for three times and washed once with anhydrous ethanol. The solid was placed in a drying oven at 60°C for 12 h to obtain a light green powder, namely Tb4[Fe(CN)6]3. Then, melamine and the light green powder Tb4[Fe(CN)6]3 were placed in a ball mill at a mass ratio of 3:2 for ball milling. The ball milling conditions were: ball milling frequency 35 Hz, ball milling forward time 10 min, interval time 5 min, reverse time 10 min, and repeated three times. Then, the mixed powder obtained by ball milling was placed in a quartz boat, and the quartz boat was placed in a tube furnace, and argon gas was introduced for protection. The argon gas flow rate was 30 mL / min, the calcination temperature was 500°C, the calcination holding time was 5 h, and the heating rate was 5°C / min. After the calcination, the product was taken out of the tube furnace to obtain a Tb-Fe composite nitrogen-carbon combustion rate catalyst derived from terbium ferrocyanate / melamine, recorded as Tb-NCM / g-C3N4. Figure 1 It can be seen that the obtained combustion rate catalyst is a hexagonal composite two-dimensional flocculent structure.

[0022] Example 2

[0023] In this example, an equal molar amount of Sm(NO3)3·6H2O is used to replace Tb(NO3)3·6H2O in Example 1, and the other steps are the same as in Example 1 to obtain a samarium ferrocyanate / melamine-derived Sm-Fe composite nitrogen-carbon combustion rate catalyst, recorded as Sm-NCM / g-C3N4.

[0024] Example 3

[0025] In this example, an equimolar amount of Eu(NO3)3·6H2O is used to replace Tb(NO3)3·6H2O in Example 1, and the other steps are the same as in Example 1 to obtain a Eu-Fe composite nitrogen-carbon combustion rate catalyst derived from europium ferrocyanate / melamine, which is recorded as Eu-NCM / g-C3N4.

[0026] Example 4

[0027] In this example, an equal molar amount of Dy(NO3)3·6H2O is used to replace Tb(NO3)3·6H2O in Example 1, and the other steps are the same as in Example 1 to obtain a Dy-Fe composite nitrogen-carbon combustion rate catalyst derived from dysprosium ferrocyanate / melamine, which is recorded as Dy-NCM / g-C3N4.

[0028] Comparative Example 1

[0029] 90.6 mg (0.02 mmol) of Tb(NO3)3·6H2O was added to 30 mL of water to obtain a saturated aqueous solution of Tb(NO3)3. 96.8 mg (0.02 mmol) of Na4[Fe(CN)6]·10H2O was added to 20 mL of water to obtain a saturated aqueous solution of Na4[Fe(CN)6]. The saturated aqueous solution of Tb(NO3)3 was then added dropwise to the saturated aqueous solution of Na4[Fe(CN)6] using a dropper. The mixture was stirred at 350 rpm for 2 h at room temperature to react and a light green suspension was obtained. The centrifuge speed was adjusted to 10000 rpm and the centrifugation time was adjusted to 10000 rpm. The obtained suspension was separated into solid and liquid, washed repeatedly with deionized water for three times, washed once with anhydrous ethanol, and the obtained solid was placed in a drying oven at 60°C for 12 hours to obtain a light green powder, namely Tb4[Fe(CN)6]3; the obtained powder was then placed in a quartz boat, and the quartz boat was placed in a tubular furnace, and argon gas was introduced for protection. The argon gas flow rate was 30 mL / min, the calcination temperature was 500°C, the calcination holding time was 5 hours, the heating rate was 5°C / min, and the product was taken out from the tubular furnace after the calcination was completed to obtain a Tb-Fe composite nitrogen-carbon combustion rate catalyst derived from terbium ferrocyanate, recorded as Tb-NCM.

[0030] Comparative Example 2

[0031] In this comparative example, an equal molar amount of Sm(NO3)3·6H2O is used to replace the Tb(NO3)3·6H2O in comparative example 1, and the other steps are the same as those in comparative example 1 to obtain a Sm-Fe composite nitrogen-carbon combustion rate catalyst derived from samarium ferrocyanate, which is recorded as Sm-NCM.

[0032] Comparative Example 3

[0033] In this comparative example, an equal molar amount of Eu(NO3)3·6H2O is used to replace the Tb(NO3)3·6H2O in comparative example 1, and the other steps are the same as those in comparative example 1 to obtain a Eu-Fe composite nitrogen-carbon combustion rate catalyst derived from europium ferrocyanate, which is recorded as Eu-NCM.

[0034] Comparative Example 4

[0035] In this comparative example, an equal molar amount of Dy(NO3)3·6H2O is used to replace the Tb(NO3)3·6H2O in comparative example 1, and the other steps are the same as those in comparative example 1 to obtain a Dy-Fe composite nitrogen-carbon combustion rate catalyst derived from dysprosium ferrocyanate, which is recorded as Dy-NCM.

[0036] Comparative Example 5

[0037] 50 mg of melamine was placed in a quartz boat, and then the quartz boat was placed in a tubular furnace. Argon gas was introduced for protection. The argon gas flow rate was 30 mL / min, the calcination temperature was 500°C, the calcination holding time was 5 h, and the heating rate was 5°C / min. After the calcination was completed, the product was taken out of the tubular furnace to obtain graphite phase carbon nitride, recorded as g-C3N4.

[0038] In order to demonstrate the beneficial effects of the present invention, 5 wt.% of the burning rate catalyst prepared in Examples 1 to 4 was added to AP to carry out combustion catalytic performance tests. The results are shown in FIG. Figure 2 At the same time, the combustion catalytic performance of the burning rate catalysts prepared in Comparative Examples 1 to 5 was compared and the results are shown in Figure 3 .

[0039] from Figure 2 It can be seen that in the heat release process of pure AP, the high temperature decomposition peak temperature is relatively late, and the apparent heat release is small. Under the same conditions, when 5wt.% of the rare earth ferrocyanate / melamine derived multi-metal composite nitrogen-carbon combustion rate catalyst in Examples 1 to 4 is added to the solid propellant main component AP, the peak temperature of the AP high temperature decomposition stage is reduced from 402.3℃ to 297.9℃, 320.8℃, 319.8℃, and 314.7℃, respectively, and the apparent decomposition heat of AP is reduced from 679.81kJ·g -1 Increased to 1601.05 kJ·g -1 、1552.92kJ·g -1 、1507.89kJ·g -1 、1578.39kJ·g -1 , respectively increased by 921.24 kJ·g -1 、873.11kJ·g -1 、828.08kJ·g -1 、898.58kJ·g -1 , among which the burning rate catalyst Tb-NCM / g-C3N4 of Example 1 has the highest degree of advance of the high temperature decomposition peak temperature of AP, and the most concentrated heat release, and the largest increase in the apparent decomposition heat of AP. This shows that after adding 5wt.% of the rare earth ferrocyanate / melamine derived multi-metal composite nitrogen-carbon burning rate catalyst of Examples 1 to 4 to AP, there is a significant catalytic effect on the decomposition of AP, which makes the AP decomposition peak temperature move forward and the heat release significantly increase at the same time.

[0040] from Figure 3 It can be seen that under the same conditions, after adding 5wt.% of the rare earth ferrocyanate-derived multi-metal nitrogen-carbon combustion rate catalyst in Comparative Examples 1 to 4 and g-C3N4 in Comparative Example 5 to the solid propellant main component AP, the decomposition peak temperature of AP is significantly reduced, and the high-temperature decomposition peak temperature of AP is reduced from 402.3℃ to 311.5℃, 322.8℃, 317.4℃, and 320.7℃, respectively, and the apparent decomposition heat of AP is reduced from 679.81kJ·g -1 Increased to 1493.40 kJ·g -1 、1202.63kJ·g -1 、1351.83kJ·g -1 、1391.76kJ·g -1 , respectively increased by 813.59 kJ·g -1 , 522.82 kJ·g -1 、672.02kJ·g -1 、711.95kJ·g -1 , which is significantly better than the test results of pure AP itself, but compared with the catalytic effect of Tb-NCM / g-C3N4 in Example 1, its AP decomposition peak temperature is relatively late and the heat release is relatively low.

[0041] In summary, the catalytic effects of the rare earth ferrocyanate / melamine derived multi-metal nitrogen-carbon burning rate catalyst in the above Examples 1 to 4, the rare earth ferrocyanate derived nitrogen-carbon burning rate catalyst in Comparative Examples 1 to 4, and the g-C3N4 in Comparative Example 5 on AP were compared, and it was found that the exothermic peak of the Tb-Fe composite nitrogen-carbon burning rate catalyst derived from terbium ferrocyanate / melamine was sharper, the exothermic release was more concentrated and the heat release was greater, and the peak temperature advance of the high-temperature decomposition peak was greater. In summary, the catalytic effect of the burning rate catalyst prepared by adding 5wt.% of Examples 1 to 4 to AP is significantly better than the composite burning rate catalyst described in Comparative Examples 1 to 4 and g-C3N4 itself.

Claims

1. A rare earth ferrocyanate / melamine derived multi-metal composite nitrogen-carbon combustion rate catalyst, characterized in that: The burning rate catalyst is a multi-metal composite nitrogen-carbon material with g-C3N4 as a carrier to load Fe and rare earth metal particles, obtained by ball-milling rare earth ferrocyanate and melamine and then calcining under inert gas protection; The rare earth ferrocyanate is selected from any one of Sm4[Fe(CN)6]3, Eu4[Fe(CN)6]3, Tb4[Fe(CN)6]3, and Dy4[Fe(CN)6]3.

2. The rare earth ferrocyanate / melamine derived multi-metal composite nitrogen-carbon combustion rate catalyst according to claim 1, characterized in that: The mass ratio of the rare earth ferrocyanate to melamine is 1:1-4.

3. The rare earth ferrocyanate / melamine derived composite nitrogen-carbon combustion rate catalyst according to claim 1, characterized in that: The mass ratio of the rare earth ferrocyanate to melamine is 1:1.5-2.

4. The rare earth ferrocyanate / melamine derived multi-metal composite nitrogen-carbon combustion rate catalyst according to any one of claims 1 to 3, characterized in that: A saturated aqueous solution of a soluble salt of a rare earth metal is added dropwise to a saturated aqueous solution of Na4[Fe(CN)6], and the reaction is carried out at room temperature for 1.5 to 4 hours, and then the obtained suspension is subjected to solid-liquid separation, and the solid is washed and dried to obtain rare earth ferrocyanide; The soluble salt of the rare earth metal is selected from any one of Sm(NO3)3·6H2O, Eu(NO3)3·6H2O, Tb(NO3)3·6H2O, and Dy(NO3)3·6H2O.

5. The rare earth ferrocyanate / melamine derived multi-metal composite nitrogen-carbon combustion rate catalyst according to claim 4, characterized in that: The molar ratio of the rare earth metal element in the soluble salt of Na4[Fe(CN)6] and the rare earth metal is 1-2:

1.

6. The rare earth ferrocyanate / melamine derived multi-metal composite nitrogen-carbon combustion rate catalyst according to claim 1, characterized in that: The frequency of the ball mill is 25-50 Hz, the forward rotation time of the ball mill is 5-30 minutes, the interval time is 5 minutes, the reverse rotation time is 5-30 minutes, and the cycle is repeated three times.

7. The rare earth ferrocyanate / melamine derived multi-metal composite nitrogen-carbon combustion rate catalyst according to claim 1, characterized in that: The frequency of the ball mill is 35-40 Hz, the forward rotation time of the ball mill is 10-15 minutes, the interval time is 5 minutes, the reverse rotation time is 10-15 minutes, and the cycle is repeated three times.

8. The rare earth ferrocyanate / melamine derived multi-metal composite nitrogen-carbon combustion rate catalyst according to claim 1, characterized in that: The calcination temperature is 300-800° C., the heat preservation time is 1-8 hours, and the heating rate is 1-10° C. / min.

9. The rare earth ferrocyanate / melamine derived multi-metal composite nitrogen-carbon combustion rate catalyst according to claim 1, characterized in that: The calcination temperature is 450-550° C., the heat preservation time is 4-6 hours, and the heating rate is 5-6° C. / min.

10. The rare earth ferrocyanate / melamine derived multi-metal composite nitrogen-carbon combustion rate catalyst according to claim 1, characterized in that: The inert gas is argon.

Citation Information

Patent Citations

  • g-C3N4 / Fe2O3 composite material and its preparation method and use

    CN105289692A

  • Preparation method of nitrogen-doped porous carbon material and solid propellant

    CN117142453A

  • Multi-metal composite nitrogen-doped carbon burning rate catalyst derived from transition metal doped rare earth ferrocyanate

    CN118788373A

  • Method for synthesizing multiple oxide of rare earth element and other element

    JP1994135722A

  • A method of making a siloxane polymer composition

    WO2015193558A1