Stable water-soluble Pt (IV) complex as well as preparation method and application thereof

By preparing the stable water-soluble Pt(IV) complex trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH, the problem of insufficient carbon deposit and water solubility of the existing platinum catalyst precursor is solved. It achieves efficient catalyst performance and feasibility of industrial production.

CN118930422APending Publication Date: 2024-11-12YUNNAN PRECIOUS METALS LAB CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410997872.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing platinum catalyst precursors have problems of carbon deposits and insufficient water solubility in their applications, which cannot meet the performance requirements of modern platinum catalysts.

Method used

Using the stable water-soluble Pt(IV) complex trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH, the precipitate is generated by reaction with malonic acid and obtained by suitable synthesis routes and conditions. High yield Pt(IV) complexes are used to prepare oxidized platinum catalysts.

Benefits of technology

It effectively reduces the carbon deposit behavior, improves water solubility and catalyst stability, avoids adverse effects on catalytic performance, and the synthesis method is simple and controllable, suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930422A_ABST
    Figure CN118930422A_ABST
Patent Text Reader

Abstract

The invention discloses a stable water-soluble Pt (IV) complex as well as a preparation method and application thereof, and belongs to the technical field of chemical catalysis. The preparation method comprises the following steps: reacting trans-[Pt (NH3) 5 (OH)] (CH3COO) 3 with malonic acid, collecting and washing the generated precipitate, reheating, dissolving in water, boiling, naturally cooling to separate out a Pt (IV) complex with the molecular formula of trans-[Pt (NH3) 4 (OH) 2] (HCOO) 2.2 HCOOH, forming a hydrogen bond ring by each pair of HCOO- / HCOOH in the Pt (IV) complex molecule through two hydrogen bonds between the head and the tail, and preparing the Pt (IV) complex by using two HCOO-.HCOOH hydrogen bond rings as external anions. Four ammonia and two hydroxyls are used as coordination inner boundaries to form a hexa-coordinated octahedral coordination cation trans-[Pt (NH3) 4 (OH)] 2 +, and trans-represents that the two hydroxyls are located at the anti-positions. The Pt (IV) complex does not contain chlorine, sulfur, phosphine, sodium, potassium, nitrate and other elements which have toxic effects on the catalyst, is high in water solubility and stability, and can be used as a catalytic precursor for preparing the diesel vehicle oxidized platinum catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical catalysis, and specifically relates to a stable water-soluble Pt (IV) complex and a preparation method and application thereof. Background Art

[0002] Platinum compounds have excellent catalytic activity and play an important role in a variety of chemical reactions, including but not limited to hydrogenation, isomerization, cyclization, dehydration, dehalogenation, oxidation, cracking and other reactions. They are the main source of catalyst active components and play a decisive role in the performance of the prepared platinum catalyst. Therefore, it is very important to select a platinum compound that matches the catalyst requirements as a catalytic precursor. In current industrial applications, the platinum catalytic precursors used are mainly traditional platinum compounds, such as N2PtCl6 (N + =H + , Na + , K + etc.), Pt(NO3)2 (10% nitric acid solution) and [Pt(NH3)4]X2 (X=NO3 - 、CH3COO - However, these compounds have obvious defects in practical applications and cannot meet the performance requirements of modern platinum catalysts.

[0003] Platinum has a unique d-electron structure and can form a variety of platinum complexes with ligands containing nitrogen and oxygen. Common platinum complexes are mainly divided into Pt(Ⅱ) complexes and Pt(Ⅳ) complexes. 8 Electronic configuration of Pt 2+ As the center, through dsp 2 The hybrid orbital bonds with the ligand to form a planar square structure; while the Pt(Ⅳ) complex belongs to d 6 The electronic configuration is an octahedral structure, in which Pt 4+ Center through d 2 sp 3 Hybrid orbitals bind to ligands. Compared with Pt(Ⅱ) complexes, Pt(Ⅳ) complexes have more stable structures, axial ligands are easy to regulate the physical and chemical properties of the complexes, and the prepared platinum catalyst metal particles have higher dispersion. These characteristics provide broader prospects for the application of platinum(Ⅳ) complexes in the field of chemical catalysis.

[0004] In recent years, the new Pt(IV) complexes reported to be synthesized are mainly trans-[Pt(NH3)4(OH)2]X2 and trans-[Pt(NH3)4(OR)(OR')]X2 (at least one of OR and OR' is a carboxylate). Among them, the trans-[Pt(NH3)4(OH)2]X2 type complexes reported in patents ZL202110524954.2 and ZL201910062506.8 have obvious deficiencies in application. For example, when X - =RCOO - (R=CH3, CH3CH(OH), CH3CH2, etc.), due to X - The carbon content is high and its oxidation products are complex, which leads to the carbon deposition phenomenon of the prepared platinum catalyst. - =OH - 、NO3 - 、H2PO4 - When the solubility of the complex in water is very low, it cannot meet the water solubility requirements of the high-platinum-loaded catalyst for the precursor. Therefore, it is necessary to find a stable Pt(IV) complex with weak carbon deposition behavior and certain water solubility. Summary of the invention

[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a stable water-soluble Pt (IV) complex and a preparation method and application thereof.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A stable water-soluble Pt(Ⅳ) complex has the molecular formula of trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH. - / HCOOH forms a hydrogen bond ring through two hydrogen bonds between the head and tail. The Pt(Ⅳ) complex is composed of two HCOO - The HCOOH hydrogen bond ring is the external anion, and the four amines and two hydroxyls are the internal coordination boundaries, forming a hexacoordinated, octahedral coordinated cation trans-[Pt(NH3)4(OH)] 2+ , trans- means that the two hydroxyl groups are in the trans position, and the chemical structure of the Pt(Ⅳ) complex is:

[0008]

[0009] A method for preparing a stable water-soluble Pt(IV) complex comprises the following steps: dissolving trans-[Pt(NH3)5(OH)](CH3COO)3 in water, adding a saturated aqueous solution of malonic acid to react and generate a precipitate, collecting and washing the precipitate, reheating and dissolving it in water and boiling it, and then naturally cooling it to room temperature to precipitate the target Pt(IV) complex.

[0010] The synthetic route of Pt(Ⅳ) complex is as follows:

[0011]

[0012] As a preferred embodiment of the present invention, the temperature of the reaction of trans-[Pt(NH3)5(OH)](CH3COO)3 and malonic acid is 40-60°C and the reaction time is 4 hours.

[0013] As a preferred embodiment of the present invention, the molar ratio of trans-[Pt(NH3)5(OH)](CH3COO)3 to malonic acid is 1:(1.05-1.2).

[0014] As a preferred embodiment of the present invention, the boiling temperature is 100-180° C. and the boiling time is 2-8 hours.

[0015] The present invention also claims to protect the Pt(IV) complex as a catalytic precursor for preparing an oxidative platinum catalyst.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] (1) The present invention combines formic acid with a cation trans-[Pt(NH3)4(OH)2] 2+ The complex not only effectively reduces the carbon deposition of traditional platinum catalysts, but also has a certain water solubility. - The HCOOH hydrogen-bonded ring as an external anion solves the problem of the chemical structure instability of the trans-[Pt(NH3)4(OH)2](HCOO)2 complex itself due to the strong reducing property of formic acid.

[0018] (2) The Pt(IV) complex prepared by the present invention does not contain elements that are poisonous to the catalyst, such as chlorine, sulfur, phosphorus, sodium, potassium, nitrate, etc., and will not have an adverse effect on the catalytic performance of the catalyst. Moreover, the Pt(IV) complex has high water solubility and high stability of the aqueous solution. Even if heated to boiling, it will not decompose to produce insoluble matter. In addition, the Pt(IV) complex prepared by the present invention is an ionic compound, which undergoes a dissociation reaction in an aqueous solution to release a stable complex cation trans-[Pt(NH3)4(OH)2] 2+, can be effectively adsorbed on the negatively charged carrier surface, which is beneficial to the catalyst loading process.

[0019] (3) The present invention synthesizes trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH through a suitable synthesis route and raw materials, with a synthesis rate of more than 95%, and a low platinum content in the waste liquid, which fundamentally solves the problems of difficulty in recovering platinum from the waste liquid and high production cost. In addition, the preparation method of the Pt(IV) complex of the present invention is simple and the synthesis is controllable, which is suitable for the batch and industrial production of trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the spatial structure diagram of trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH.

[0021] Figure 2 This is the thermal decomposition curve (TG-DTA) of trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH prepared in Example 1 in simulated air.

[0022] Figure 3 This is the thermal decomposition curve (TG-DTA) of trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH prepared in Example 1 in nitrogen.

[0023] Figure 4 4a is the conversion efficiency curve of CO oxidation of the two platinum catalysts in fresh and aged states in Example 4, where 4a is the fresh state and 4b is the aged state.

[0024] Figure 5 5a is the conversion efficiency curve of C3H6 oxidation of the two platinum catalysts in fresh and aged states in Example 4, where 5a is the fresh state and 5b is the aged state.

[0025] Figure 6 6a is the conversion efficiency curve of the two platinum catalysts in Example 4 for oxidizing NO to NO2 in fresh and aged states, where 6a is the fresh state and 6b is the aged state.

[0026] In the figure, Pt-NF is a catalyst in a fresh state prepared by the excess impregnation method of platinum nitrate, and Pt-NA is a catalyst in an aged state prepared by the excess impregnation method of platinum nitrate; Pt-CF is a catalyst in a fresh state prepared by the excess impregnation method of Pt(IV) complex, and Pt-CA is a catalyst in an aged state prepared by the excess impregnation method of Pt(IV) complex. DETAILED DESCRIPTION

[0027] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0028] Example 1

[0029] The preparation method of trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH comprises the following steps:

[0030] At 50°C, 5.05 g (10.65 mmol) of trans-[Pt(NH3)5(OH)](CH3COO)3 was dissolved in 20 mL of water to form a clear solution. 8 mL of a saturated aqueous solution of HOOCCH2COOH (1.33 g, 12.78 mmol) was added dropwise to the clear solution, and a white precipitate was immediately precipitated. After the addition was completed, the reaction solution was stirred and reacted at 50°C for 4 hours, then cooled to room temperature, the white precipitate was collected by filtration, washed with ice water 3 times and anhydrous ethanol once, and dried. The obtained white precipitate was reheated and dissolved in water, boiled at 160°C for 6 hours, and then naturally cooled to room temperature to precipitate colorless crystals. The colorless crystals were collected by filtration, namely trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH (4.85 g) with a yield of 95.04%.

[0031] Structural characteristic parameters: <1> Elemental analysis: Measured values ​​Pt 40.55%, C 9.88%, H 4.69%, N 11.08% (calculated values ​​Pt 40.71%, C 10.02%, H 4.18%, N 11.69%; <2> 1 H NMR(500MHz,DMSO-d6)δ8.30(s,4H,2 H COO - +2 H COOH), 6.04-4.92(m,12H,4N H 3),3.32(s,D2O),2.49(t,J=2.2Hz,DMSO),-0.01(s,TMS); <3> 13 C NMR(126MHz,DMSO-d6)δ176.22(4C,2H C OO - +2H COOH),39.52(dt,J=42.6,21.4Hz,DMSO); <4> 3393(m),3290(m),3193(m),1717(s),1592(s),1537(s),1482(s),538(w),495(w); <5> FAB + -MS:480[MH] + ; 342[M-HCOO-2HCOOH] + ; <5> The single crystal of the complex was prepared by solvent evaporation method, and the crystal structure of the complex was obtained by X-ray single crystal diffraction analysis. Figure 3 As shown, the cation trans-[Pt(NH3)4(OH)2] 2+ It is a six-coordinated octahedral configuration. Each pair of HCOO - / HCOOH forms a hydrogen bond ring through the head-to-tail hydrogen bond, and the complex is HCOO - The HCOOH hydrogen bond ring is an external anion. These parameters are consistent with the chemical structure of the Pt(IV) complex of the present invention (see the chemical spatial structure). Figure 1 ).

[0032] like Figure 2 and 3 It can be seen that the Pt(IV) complex prepared in Example 1 can undergo thermal decomposition reaction at a relatively low temperature (<300°C) in air or nitrogen atmosphere to generate metal platinum. The thermal decomposition temperature range is relatively narrow (<200°C), which is conducive to energy saving in the thermal reduction or calcination process of catalyst preparation. Its thermal decomposition reaction is:

[0033]

[0034] Example 2

[0035] The preparation method of trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH comprises the following steps:

[0036] At 60°C, 5.05 g (10.65 mmol) of trans-[Pt(NH3)5(OH)](CH3COO)3 was dissolved in 20 mL of water to form a clear solution. 8 mL of a saturated aqueous solution of HOOCCH2COOH (1.16 g, 11.18 mmol) was added dropwise to the clear solution, and a white precipitate was immediately precipitated. After the addition was completed, the reaction solution was stirred and reacted at 60°C for 4 hours, then cooled to room temperature, the white precipitate was collected by filtration, washed with ice water 3 times and anhydrous ethanol once, and dried. The obtained white precipitate was reheated and dissolved in water, boiled at 180°C for 2 hours, and then naturally cooled to room temperature to precipitate colorless crystals. The colorless crystals were collected by filtration, namely trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH (4.16 g) with a yield of 81.51%.

[0037] Example 3

[0038] The preparation method of trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH comprises the following steps:

[0039] At 40°C, 5.05 g (10.65 mmol) of trans-[Pt(NH3)5(OH)](CH3COO)3 was dissolved in 20 mL of water to form a clear solution. 8 mL of a saturated aqueous solution of HOOCCH2COOH (1.22 g, 11.72 mmol) was added dropwise to the clear solution, and a white precipitate was immediately precipitated. After the addition was completed, the reaction solution was stirred and reacted at 40°C for 4 hours, then cooled to room temperature, the white precipitate was collected by filtration, washed with ice water 3 times and anhydrous ethanol once, and dried. The obtained white precipitate was reheated and dissolved in water, boiled at 130°C for 6 hours, and then naturally cooled to room temperature to precipitate colorless crystals. The colorless crystals were collected by filtration, namely trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH (4.52 g) with a yield of 88.57%.

[0040] Example 4

[0041] Preparation of diesel vehicle oxidation catalyst using the Pt(IV) complex prepared in Example 1 of the present invention as a precursor and performance evaluation:

[0042] Alumina was selected as a carrier, and commercially available platinum nitrate (in the form of a 10% nitric acid solution) and the Pt(IV) complex trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH of the present invention were used as precursors. Two catalysts with a platinum loading of 1.3% were prepared by an excess impregnation method, which were numbered Pt-N (control catalyst) and Pt-C, respectively. The fresh sample (fresh) was calcined at 550°C for 3 hours to ensure that the noble metal precursor was completely decomposed. The aged sample (aged) was calcined at 700°C for 10 hours.

[0043] A multi-pipeline continuous micro fixed bed reactor is used, with a gas space velocity (Sv) of 80,000 h -1 The specific test conditions are listed in Table 1. The catalyst was pressed into tablets, and about 0.5 grams of the sample was weighed and loaded into the reaction tube. The temperature was programmed from 100°C to 500°C. The concentrations of CO, C3H6, NO, NO2, and N2O before and after the reactor at different temperatures were detected online by the American MKS2030 series Fourier transform infrared spectrometer to investigate the oxidation ability of the catalyst for CO, C3H6, and NO, and to evaluate the activity of the catalyst.

[0044] Table 1

[0045] gas NO CO <![CDATA[C3H6]]> <![CDATA[C3H8]]> <![CDATA[O2]]> <![CDATA[H2O]]> <![CDATA[N2]]> Volume fraction <![CDATA[500×10 -6 ]]> <![CDATA[500×10 -6 ]]> <![CDATA[200×10 -6 ]]> <![CDATA[100×10 -6 ]]> 8% 10% Balance gas

[0046] like Figure 4-5 It can be seen that in the fresh state, the oxidation curve of CO and C3H6 of the catalyst Pt-C prepared by the Pt(Ⅳ) complex of the present invention is closer to the low temperature region, indicating that the oxidation ability of the catalyst Pt-C prepared by the Pt(Ⅳ) complex to CO and C3H6 is better than that of Pt-N; although in the low temperature region (225-300°C), the ability of the Pt-C catalyst to oxidize NO to generate NO2 is lower than that of Pt-N, but the NO2 / NO ratio obtained by the highest oxidation efficiency is x The maximum percentage value is better than that of Pt-N catalyst.

[0047] In the aged state, the oxidation ability of Pt-C catalyst for CO is equivalent to that of Pt-N, the oxidation ability for C3H6 is better than that of Pt-N, and the oxidation ability for NO is consistent with that of Pt-N. However, the NO2 / NO ratio obtained by the highest oxidation efficiency is x The maximum percentage value is better than Pt-N. Therefore, the catalyst prepared using the Pt(IV) complex of the present invention as a precursor has better oxidation ability for CO, C3H6 and NO than platinum nitrate, and can be used to prepare oxidation-type platinum catalysts for diesel vehicles, showing good commercial application prospects.

[0048] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A stable water-soluble Pt(IV) complex, characterized in that: The molecular formula is trans-[Pt(NH3)4(OH)2](HCOO)2·2HCOOH. Each pair of HCOO in the Pt(Ⅳ) complex molecule - / HCOOH forms a hydrogen bond ring through two hydrogen bonds between the head and tail. The Pt(Ⅳ) complex is composed of two HCOO - The HCOOH hydrogen bond ring is the external anion, and the four amines and two hydroxyls are the internal coordination boundaries, forming a hexacoordinated, octahedral coordinated cation trans-[Pt(NH3)4(OH)] 2+ , trans- means that the two hydroxyl groups are in the trans position, and the chemical structure of the Pt(Ⅳ) complex is:

2. The method for preparing a stable water-soluble Pt(IV) complex according to claim 1, characterized in that: The method comprises the following steps: dissolving trans-[Pt(NH3)5(OH)](CH3COO)3 in water, adding a saturated aqueous solution of malonic acid to react and generate a precipitate, collecting and washing the precipitate, reheating and dissolving it in water and boiling it, and then naturally cooling it to room temperature to precipitate the target Pt(IV) complex.

3. The method for preparing a stable water-soluble Pt(IV) complex according to claim 2, characterized in that: The reaction temperature of the trans-[Pt(NH3)5(OH)](CH3COO)3 and malonic acid is 40-60°C and the reaction time is 4 hours.

4. The method for preparing a stable water-soluble Pt(IV) complex according to claim 2, characterized in that: The molar ratio of trans-[Pt(NH3)5(OH)](CH3COO)3 to malonic acid is 1:(1.05-1.2).

5. The method for preparing a stable water-soluble Pt(IV) complex as claimed in claim 2, characterized in that: The boiling temperature is 100-180° C. and the boiling time is 2-8 hours.

6. The stable water-soluble Pt(IV) complex as claimed in claim 1 is used as a catalytic precursor for preparing an oxidative platinum catalyst.