Acrylic resin polymer as well as preparation method and application thereof

By designing the topological structure and synthesis method of acrylic resins, the problem of unchanged main chain length in photolithography of traditional polymers is solved, the photolithography sensitivity and pattern edge fineness are improved, and the molecular weight controllability and molecular weight distribution are achieved. The narrowing of the photoresist improves the performance of the photoresist.

CN118930715AActive Publication Date: 2024-11-12NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310544532.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

The length of the main chain remains unchanged during the photolithography process, resulting in insufficient photolithography sensitivity and pattern edge roughness, and the exposure energy increases pattern edge roughness, making it difficult to meet the solubility changes of photoresist during the development process.

Method used

Using the preparation method of acrylic resin polymers, a two-arm, three-arm or four-arm topological polymerization reaction is carried out by performing reversible-inactivated radical polymerization reaction catalyzed by metal or metal salt in an inert gas atmosphere, The halogen initiator is used as the initiator for radical polymerization to synthesize the methacrylic resin containing acetal groups on the backbone to control its molecular weight and molecular weight distribution.

Benefits of technology

The photolithographic sensitivity of the resin is improved, the controllability of molecular weight and the narrowing of molecular weight distribution are achieved, which conforms to the characteristics of active radical polymerization and improves the performance of photoresist.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930715A_ABST
    Figure CN118930715A_ABST
Patent Text Reader

Abstract

The invention discloses an acrylic resin polymer as well as a preparation method and application thereof. The acrylic resin polymer has a structure as shown in a formula (I): # imgabs0 #, wherein x is equal to 1 to 1600; r1 is selected from residues of dihydric alcohol or dihydric phenol, residues of trihydric alcohol or trihydric phenol and residues of tetrahydric alcohol or tetrahydric phenol, and n is larger than or equal to 2; r2 is selected from residues of dihydric alcohol or dihydric phenol; r3 is selected from methyl or hydrogen atom; r4 is selected from halogen bromine atoms or chlorine atoms; and R5 is selected from any one of benzyl, adamantyl or hydroxyl substituted adamantyl, C1-C12 alkyl or hydroxyl substituted C1-C12 alkyl, and glycidyl. The polymer provided by the invention has main chain stimulated fracture and a topological structure of a two-arm type, three-arm type or four-arm type, and the structural design characteristic is beneficial to improving the resin photoetching sensitivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer preparation, and specifically relates to an acrylic resin polymer and a preparation method and application thereof. Background Art

[0002] The molecular weight and molecular weight distribution characteristics of polymers are important indicators of resins in practical applications. In photoresists, the molecular weight of polymers determines the performance of photoresists. In the development process of positive photoresists, methacrylic resins are mostly achieved by breaking the chemical bonds of the groups on the polymer side chains to change the solubility of the polymer in the developer. In this process, the photoresist requires that the polymer must have a certain molecular weight to obtain a fine pattern. Since the main chain length (degree of polymerization) of the polymer does not change before and after photolithography, the side chain groups of the polymer need to have a higher photolithography response sensitivity and produce enough hydrophilic groups to achieve the dissolution of the polymer in the developer. However, the number of chemical bond breaks caused by a constant exposure dose is limited. In order to meet the change in the solubility of the photoresist, only the exposure energy can be increased, which increases the requirements for the photolithography machine. At the same time, the excessive length of the polymer main chain will also increase the roughness of the pattern edge. Therefore, in order to avoid the adverse factors caused by the change in the solubility of the resin before and after photolithography, the molecular weight of the polymer needs to be controlled within a narrow window.

[0003] In summary, the main chain length (degree of polymerization) of traditional polymers does not change before and after photolithography, which affects the photolithography sensitivity and pattern edge roughness to a certain extent. Summary of the invention

[0004] The main purpose of the present invention is to provide an acrylic resin polymer and a preparation method and application thereof, so as to overcome the deficiencies in the prior art.

[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0006] The present invention provides an acrylic resin polymer having a structure as shown in formula (I):

[0007]

[0008] wherein x=1-1600; R1 is selected from the residue of a diol or a dihydric phenol, the residue of a triol or a trihydric phenol, the residue of a tetraol or a tetrahydric phenol, and n≥2; R2 is selected from the residue of a diol or a dihydric phenol; R3 is selected from a methyl group or a hydrogen atom; R4 is selected from a halogen bromine atom or a chlorine atom; R5 is selected from any one of a benzyl group, an adamantyl group or a hydroxy-substituted adamantyl group, a C1-C12 alkyl group or a hydroxy-substituted C1-C12 alkyl group, and a glycidyl group;

[0009] The molecular weight of the acrylic resin polymer is 1000 to 200000 g / mol, and the molecular weight distribution is 1.04 to 2.50;

[0010] Preferably, R1 is selected from the residue of a dihydric alcohol or a dihydric phenol, and n is 2, or, R1 is selected from the residue of a trihydric alcohol or a trihydric phenol, and n is 3, or, R1 is selected from the residue of a tetrahydric alcohol or a tetrahydric phenol, and n is 4.

[0011] The present invention also provides a method for preparing the aforementioned acrylic resin polymer, comprising:

[0012] In an inert gas atmosphere, an acrylate monomer or a methacrylate monomer, a halogen initiator, a catalyst and a ligand are subjected to a metal or metal salt-catalyzed reversible-deactivated free radical polymerization reaction in a solvent at 0 to 110° C. to obtain the acrylic resin polymer;

[0013] Wherein, the halogen initiator has a structure as shown in formula (II):

[0014]

[0015] R1 is selected from the residue of a diol or a dihydric phenol, the residue of a triol or a trihydric phenol, the residue of a tetraol or a tetrahydric phenol, and n≥2; R2 is selected from the residue of a diol or a dihydric phenol; R3 is selected from a methyl group or a hydrogen atom; R4 is selected from a halogen bromine atom or a chlorine atom;

[0016] Preferably, R1 is selected from the residue of a dihydric alcohol or a dihydric phenol, and n is 2, or, R1 is selected from the residue of a trihydric alcohol or a trihydric phenol, and n is 3, or, R1 is selected from the residue of a tetrahydric alcohol or a tetrahydric phenol, and n is 4.

[0017] Furthermore, the molar ratio of the acrylic acid ester monomer or methacrylic acid ester monomer, the halogen initiator, the catalyst and the complexing agent is (1-1600):1:(0.05-10):(0.15-15).

[0018] The present invention also provides the use of the aforementioned acrylic resin polymer in the preparation of photoresist.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) The acrylic resin polymer of the present invention is a polymer with main chain stimulated cleavage and a topological structure of two arms, three arms or four arms. This structural design feature is conducive to improving the photolithography sensitivity of the resin.

[0021] (2) The present invention utilizes a reversible-deactivated free radical polymerization method catalyzed by metal or metal salt, and designs and synthesizes a halogen-containing compound with an acetal structure as an initiator for free radical polymerization to achieve the synthesis of a polymer resin containing an acetal group in the polymer main chain, thereby preparing a methacrylic resin containing an acetal group in the main chain. The molecular weight of the resin is controllable and the molecular weight distribution is relatively narrow (Mw / Mn<1.50), which meets the characteristics of "active" free radical polymerization. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 is ethyl 2-vinyloxy-2-bromo-2-methylpropionate in one embodiment of the present application 1 H NMR test results.

[0024] Figure 2 is a bifunctional halogen initiator (II-12) in one embodiment of the present application 1 H NMR test results.

[0025] Figure 3 is a trifunctional halogen initiator (II-13) in one embodiment of the present application 1 H NMR test results.

[0026] Figure 4 is a tetrafunctional halogen initiator (I1-22) in one embodiment of the present application 1 H NMR test results.

[0027] Figure 5 It is a photolithography result diagram of methacrylic resin of Example 5, Example 6 and Comparative Example 1 in one embodiment of the present application (the line width of the mask used is 200 nanometers). DETAILED DESCRIPTION

[0028] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] One aspect of an embodiment of the present invention provides an acrylic resin polymer having a structure as shown in formula (I):

[0030]

[0031] wherein x=1-1600; R1 is selected from the residue of a diol or a dihydric phenol, the residue of a triol or a trihydric phenol, the residue of a tetraol or a tetrahydric phenol, and n≥2; R2 is selected from the residue of a diol or a dihydric phenol; R3 is selected from a methyl group or a hydrogen atom; R4 is selected from a halogen bromine atom or a chlorine atom; R5 is selected from any one of a benzyl group, an adamantyl group or a hydroxy-substituted adamantyl group, a C1-C12 alkyl group or a hydroxy-substituted C1-C12 alkyl group, and a glycidyl group;

[0032] The molecular weight of the acrylic resin polymer is 1000 to 200000 g / mol, and the molecular weight distribution is 1.04 to 2.50;

[0033] Preferably, R1 is selected from the residue of a dihydric alcohol or a dihydric phenol, and n is 2, or, R1 is selected from the residue of a trihydric alcohol or a trihydric phenol, and n is 3, or, R1 is selected from the residue of a tetrahydric alcohol or a tetrahydric phenol, and n is 4.

[0034] Another aspect of the embodiments of the present invention further provides a method for preparing the aforementioned acrylic resin polymer, comprising:

[0035] In an inert gas atmosphere, an acrylate monomer or a methacrylate monomer, a halogen initiator, a catalyst and a ligand are subjected to a metal or metal salt-catalyzed reversible-deactivated free radical polymerization reaction in a solvent at 0 to 110° C. to obtain the acrylic resin polymer;

[0036] Wherein, the halogen initiator has a structure as shown in formula (II):

[0037]

[0038] R1 is selected from the residue of a diol or a dihydric phenol, the residue of a triol or a trihydric phenol, the residue of a tetraol or a tetrahydric phenol, and n≥2; R2 is selected from the residue of a diol or a dihydric phenol; R3 is selected from a methyl group or a hydrogen atom; R4 is selected from a halogen bromine atom or a chlorine atom;

[0039] Preferably, R1 is selected from the residue of a dihydric alcohol or a dihydric phenol, and n is 2, or, R1 is selected from the residue of a trihydric alcohol or a trihydric phenol, and n is 3, or, R1 is selected from the residue of a tetrahydric alcohol or a tetrahydric phenol, and n is 4.

[0040] In some preferred embodiments, the molar ratio of the acrylic acid ester monomer or methacrylic acid ester monomer, the halogen initiator, the catalyst and the ligand is (1-1600):1:(0.05-10):(0.15-15).

[0041] In some more preferred embodiments, the molar ratio of the acrylic acid ester monomer or methacrylic acid ester monomer, the halogen initiator, the catalyst and the ligand is (20-75):1:(1-5):(2-6).

[0042] In some preferred embodiments, the acrylate monomer or methacrylate monomer can be selected from benzyl methacrylate (BzMA), methyl methacrylate (MMA), tert-butyl methacrylate (tBMA), glycidyl methacrylate (GMA), n-butyl methacrylate (nBMA), dicyclopentyl methacrylate (HDCPMA), hydroxyethyl methacrylate (HEMA), hydroxypropyl methacrylate (HPMA), 2-methyl-2-adamantyl methacrylate (MAMA), 2-ethyl-2-adamantyl methacrylate (EAMA), 1-adamantyl methacrylate Ester (ADAMA), 3-hydroxy-1-adamantyl methacrylate (HAMA), benzyl acrylate (BzA), methyl acrylate (MA), tert-butyl acrylate (tBA), glycidyl acrylate (GA), n-butyl acrylate (nBA), hydroxyethyl acrylate (HEA), hydroxypropyl acrylate (HPA), 2-methyl-2-adamantyl acrylate (MAA), 2-ethyl-2-adamantyl acrylate (EAA), 1-adamantyl acrylate (ADAA), 3-hydroxy-1-adamantyl acrylate (HAA), etc., any one or more combinations thereof, but are not limited thereto.

[0043] In some more preferred embodiments, the methacrylate monomer is a homopolymer of tert-butyl methacrylate, 2-methyl-2-adamantyl methacrylate, 1-adamantyl methacrylate, 3-hydroxy-1-adamantyl methacrylate, or a copolymer of several monomers.

[0044] In some preferred embodiments, the diol or dihydric phenol may be selected from the structures shown in any one or more of the following formulae:

[0045]

[0046] In some preferred embodiments, the trihydric alcohol or trihydric phenol may be selected from the structures shown in any one or more of the following formulae:

[0047]

[0048] In some preferred embodiments, the tetrahydric alcohol or tetrahydric phenol may be selected from the structures shown in any one or more of the following formulae:

[0049]

[0050] In some preferred embodiments, the halogen initiator is selected from one or more of the compounds represented by formula II-1 to formula II-24:

[0051]

[0052] In some preferred embodiments, the catalyst may include any one or more of copper, iron, cupric chloride, cuprous chloride, ferric bromide, ferrous bromide, cupric bromide, cuprous bromide, etc., but is not limited thereto.

[0053] In some more preferred embodiments, the catalyst is cuprous bromide.

[0054] In some preferred embodiments, the ligand may include any one or more of N,N,N′,N,′N″-pentamethyldiethylenetriamine (PMDETA), 2,2′-bipyridine (BIPY), 1,1,4,7,10,10-hexamethyltriethylenetetramine (HMTETA), etc., but is not limited thereto.

[0055] In some more preferred embodiments, the complexing agent is N,N,N′,N,′N″-pentamethyldiethylenetriamine.

[0056] In some preferred embodiments, the solvent may include any one or more of toluene, xylene, tetrahydrofuran, dioxane, ethyl acetate, etc., but is not limited thereto.

[0057] In some more preferred embodiments, the solvent is toluene.

[0058] Furthermore, when the methacrylate monomers are copolymerized, the molar ratio of tert-butyl methacrylate, 2-methyl-2-adamantyl methacrylate, 1-adamantyl methacrylate and 3-hydroxy-1-adamantyl methacrylate is (3-400):(3-400):(3-400):(3-400).

[0059] Furthermore, the molar ratio of tert-butyl methacrylate, 2-methyl-2-adamantyl methacrylate, 1-adamantyl methacrylate and 3-hydroxy-1-adamantyl methacrylate is (5-40):(5-40):(5-40):(5-40).

[0060] In a more specific implementation process, the methacrylate monomer is copolymerized with tert-butyl methacrylate, 2-methyl-2-adamantyl methacrylate, and 3-hydroxy-1-adamantyl methacrylate, the halogen initiator is compound II-13, the catalyst is cuprous bromide, and the coordination agent is N,N,N′,N,′N″-pentamethyldiethylenetriamine. A metal or metal salt-catalyzed reversible-deactivated free radical polymerization reaction is carried out in toluene at 90° C. for 24 hours, and the monomer conversion rate can reach >50%. The structural formula of the obtained polymer is as follows:

[0061]

[0062] By means of the above scheme, the resin in the present invention has at least the following advantages:

[0063] The present invention utilizes a metal or metal salt catalyzed reversible-deactivated free radical polymerization method to prepare a methacrylic resin containing acetal groups in the main chain. The molecular weight of the resin is controllable and the molecular weight distribution is relatively narrow (Mw / Mn<1.50), which meets the characteristics of "active" free radical polymerization.

[0064] Another aspect of the embodiments of the present invention further provides the use of the aforementioned methacrylic resin polymer in preparing photoresist.

[0065] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0066] In the following examples of the present invention, the raw materials and reagents used, unless otherwise specified, can be directly used after being obtained from commercial channels.

[0067] In the present invention, the following test method is adopted:

[0068] 1. The number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) of the obtained polymer were measured by TOSOH HLC-8420 gel permeation chromatograph equipped with a refractive index detector (TOSOH), the guard column used was TSK gel Super MP-N (4.6×20 mm), the detection column was TSK gel Super HZ-N (4.6×150 mm), DMF (with 0.1 wt% LiBr added as a cosolvent) was used as the eluent, the test temperature was 40°C, and the flow rate was 0.35 mL·min -1 , molecular weight range is 5×10 2 ~5×10 5g / mol. The gel permeation chromatography samples were injected using a TOSOH plus autosampler, and the results of the measured polymers were calibrated with standard PS samples purchased from TOSOH. The sample preparation process for the GPC test was as follows: the polymer was dissolved in THF at a concentration of 1 to 5 mg / mL, the polymer solution was passed through a small column of neutral alumina and a syringe equipped with a 0.45 μm filter, and finally the pure polymer solution was injected into the test bottle.

[0069] 2. The NMR spectra of the obtained products and polymers were obtained by testing with a Bruker 400 MHz NMR instrument, using DMSO-d6 as a deuterated reagent, at 25°C, with tetramethylsilane (TMS) as an internal standard.

[0070] Example 12 Synthesis of Ethyl Vinyloxy-2-Bromo-2-Methylpropionate

[0071] Under an inert gas atmosphere, vinyl glycol ether (4.00 g, 45.4 mmol) was dissolved in 100 mL of anhydrous dichloromethane, triethylamine (7.56 mL, 54.4 mmol) was added, stirred on a magnetic stirrer, and the reaction vessel was placed in an ice bath, and then a mixed solution of bromoisobutyryl bromide (5.62 mL, 45.4 mmol) and anhydrous dichloromethane (20 mL) was added dropwise, and the reaction was continued at room temperature for at least 8 h. After the reaction was completed, a yellowish transparent liquid, i.e., ethyl 2-vinyloxy-2-bromo-2-methylpropionate, was finally obtained by extraction, drying, distilling off the solvent and purifying. A total of 2.13 g, a yield of 86%, and ethyl 2-vinyloxy-2-bromo-2-methylpropionate 1 H NMR test results, such as Figure 1 As shown, it is proved that the compound 2-vinyloxy-2-bromo-2-methylpropionic acid ethyl ester is successfully synthesized with a purity of >95%.

[0072] The molecular structural formula of ethyl 2-vinyloxy-2-bromo-2-methylpropionate in this embodiment is as follows:

[0073]

[0074] Example 2 Synthesis of bifunctional halogen initiator (II-12)

[0075] Under an inert gas atmosphere, bisphenol A (1.44 g, 6.3 mmol) and 50 mL of anhydrous dichloromethane were added to a reaction flask, followed by addition of p-toluenesulfonic acid (54.3 mg, 0.3 mmol). Under ice bath conditions, a mixed solution of ethyl 2-vinyloxy-2-bromo-2-methylpropionate (3.00 g, 12.6 mmol) and 20 mL of anhydrous dichloromethane was added dropwise to the reaction mixture. After the addition was completed, the reaction mixture was stirred at room temperature for at least 12 h. After the reaction was completed, a slightly yellowish transparent liquid (3.68 g, yield 83%) was finally obtained by extraction, drying, distilling off the solvent and purifying. The slightly yellowish transparent liquid was a bifunctional halogen initiator (II-12), which 1 H NMR test results, such as Figure 2 As shown, it is proved that the bifunctional halogen initiator (II-12) was successfully synthesized with a purity of >95%.

[0076] The molecular structure of the bifunctional halogen initiator (II-12) in this embodiment is as follows:

[0077]

[0078] Example 3 Synthesis of trifunctional halogen initiator (II-13)

[0079] Under an inert gas atmosphere, 1,1,1-tri(4-hydroxyphenyl)ethane (3.44 g, 11.2 mmol) and 30 mL of anhydrous dichloromethane were added to a reaction flask, followed by addition of p-toluenesulfonic acid (56.0 mg, 0.6 mmol). Under ice bath conditions, a mixed solution of ethyl 2-vinyloxy-2-bromo-2-methylpropionate (8.00 g, 33.7 mmol) and 10 mL of anhydrous dichloromethane was added dropwise to the reaction mixture. After the addition was completed, the reaction mixture was stirred at room temperature for at least 12 h. After the reaction was completed, extraction, drying, evaporation of the solvent and purification were performed to finally obtain a slightly yellowish transparent liquid (7.88 g, yield 69%), and the slightly yellowish transparent liquid was a trifunctional halogen initiator (II-13), which 1 H NMR test results, such as Figure 3 As shown, it was proved that the trifunctional halogen initiator (II-13) was successfully synthesized with a purity of >95%.

[0080] The molecular structure of the trifunctional halogen initiator (II-13) in this embodiment is as follows:

[0081]

[0082] Example 4 Synthesis of tetrafunctional halogen initiator (II-22)

[0083] Under an inert gas atmosphere, di(trihydroxymethyl)propane (0.70 g, 2.8 mmol) and 30 mL of ethylene glycol dimethyl ether were added to a reaction flask, followed by addition of p-toluenesulfonic acid (20 mg, 0.1 mmol). Under an ice bath, ethyl 2-vinyloxy-2-bromo-2-methylpropanoate (2.66 g, 11.2 mmol) was added directly to the reaction mixture, and the reaction mixture was stirred at room temperature for at least 12 h. After the reaction was completed, extraction, drying, evaporation of the solvent and purification were performed to finally obtain a light yellow transparent liquid (1.68 g, yield 50%), and the light yellow transparent liquid was a tetrafunctional halogen initiator (II-22), which 1 HNMR test results, such as Figure 4 As shown, it was proved that the tetrafunctional halogen initiator (II-22) was successfully synthesized with a purity of >95%.

[0084] The molecular structure of the tetrafunctional halogen initiator (II-22) in this embodiment is as follows:

[0085]

[0086] Example 5 Preparation of two-arm methacrylic resin

[0087] A bifunctional halogen initiator (II-12) was used as an initiator for a metal or metal salt-catalyzed reversible-deactivated free radical polymerization, and the feed was added at a molar ratio of [tBMA]0 / [ADAMA]0 / [MAMA]0 / [HAMA]0 / [II-12]0 / [CuBr]0 / [PMDETA]0=30 / 30 / 30 / 30 / 1 / 3 / 5, tBMA (3.04 g, 21.4 mmol), ADMA (4.70 g, 21.4mmol), MAMA (5.00g, 21.4mmol), HAMA (5.05g, 21.4mmol), initiator II-12 (0.50g, 0.7mmol), CuBr (0.31g, 2.1mmol) and PMDETA (0.62g, 3.6mmol) were added to a 25mL reaction bottle dried with a magnetic stirrer, and 10mL of anhydrous toluene was added as a polymerization solvent. Then the reaction atmosphere was replaced with an inert gas through a double-row tube, and sealed and placed in a magnetic stirrer at 90°C, and the polymerization reaction was set for 24h. After the polymerization reaction was completed, the reaction mixture was taken out and diluted with 20mL tetrahydrofuran and precipitated with 500mL petroleum ether. The polymer product was collected by filtration and dried to constant weight at 30°C under vacuum. Then, the polymerization conversion was calculated according to the weight method.

[0088] The molecular structure of the two-arm methacrylic resin in this embodiment is as follows:

[0089]

[0090] Example 6 Preparation of three-arm methacrylic resin

[0091] A trifunctional halogen initiator (II-13) was used as an initiator for a metal or metal salt-catalyzed reversible-deactivated free radical polymerization, and the feed was added at a molar ratio of [tBMA]0 / [ADAMA]0 / [MAMA]0 / [HAMA]0 / [I-13]0 / [CuBr]0 / [PMDETA]0=30 / 30 / 30 / 30 / 1 / 4 / 6, tBMA (2.93 g, 20.60 mmol), ADAMA (4.55 g, 5.3 mmol), and HAMA (2.5 g, 5.3 mmol). , 20.60mmol), MAMA (4.84g, 20.60mmol), HAMA (4.88g, 20.60mmol), initiator II-13 (0.70g, 0.69mmol), CuBr (0.39g, 2.74mmol) and PMDETA (0.72g, 4.12mmol) were added to a 25mL reaction bottle equipped with a magnetic stirrer and dried, and 10mL of toluene was added as a polymerization solvent. Then the reaction atmosphere was replaced with an inert gas through a double-row tube, and sealed and placed in a magnetic stirrer at 90°C, and the polymerization reaction was set for 24h. After the polymerization reaction was completed, the reaction mixture was taken out and precipitated using 500mL of petroleum ether. The polymer product was collected by filtration and dried to constant weight at 30°C under vacuum. Then, the polymerization conversion was calculated according to the weight method.

[0092] The molecular structure of the three-arm methacrylic resin in this embodiment is as follows:

[0093]

[0094] Example 7 Preparation of Four-arm Methacrylic Resin

[0095] A tetrafunctional halogen initiator (II-22) was used as an initiator for a metal or metal salt-catalyzed reversible-deactivated free radical polymerization, and the feed was added at a molar ratio of [tBMA]0 / [ADAMA]0 / [MAMA]0 / [HAMA]0 / [II-22]0 / [CuBr]0 / [PMDETA]0=30 / 30 / 30 / 30 / 1 / 5 / 6, tBMA (100.0 mg, 0.70 mmol), ADAMA (154.9 m g, 0.70mmol), MAMA (164.8mg, 0.70mmol), HAMA (166.2mg, 0.70mmol), initiator II-22 (28.1mg, 0.02mmol), CuBr (16.8mg, 0.12mmol) and PMDETA (24.3mg, 0.14mmol) were added to a 5mL reaction bottle dried with a magnetic stirrer, and 2mL of toluene was added as the polymerization solvent. Then the reaction atmosphere was replaced with an inert gas through a double-row tube, and the mixture was sealed and placed in a magnetic stirrer at 90°C for a set polymerization time. After the polymerization reaction was completed, the reaction mixture was taken out and precipitated using 200mL of petroleum ether. The polymer product was collected by filtration and dried to constant weight at 30°C under vacuum. Then, the polymerization conversion was calculated according to the weight method.

[0096] The molecular structure of the four-arm methacrylic resin in this embodiment is as follows:

[0097]

[0098] Comparative Example 1 Preparation of conventional methacrylic resin

[0099] The resin prepared by using 2-bromoisobutyrate (EBiB) as a cuprous bromide-catalyzed reversible-deactivated free radical polymerization initiator is a comparative example, and the molar ratio of the feed is [tBMA]0 / [ADAMA]0 / [MAMA]0 / [HAMA]0 / [EBiB]0 / [CuBr]0 / [PMD ETA]0 = 30 / 30 / 30 / 30 / 1 / 1 / 2 for feeding, tBMA (3.04g, 21.4mmol), ADAMA (4.70g, 21.4mmol), MAMA (5.00g, 21.4mmol), HAMA (5.05g, 21.4mmol), EBiB (0.14g, 0.7mmol), CuBr (102.1mg, 0.7mmol) and PMDETA (0.25g, 1.4mmol) were added to a 25mL reaction bottle dried with a magnetic stirrer, and 10mL of toluene was added as a polymerization solvent. Then the reaction atmosphere was replaced with an inert gas by a double-row tube, and a magnetic stirrer was placed at 90°C after sealing, and the polymerization reaction was set for a time. After the polymerization reaction was completed, the reaction mixture was taken out and precipitated using 500mL of petroleum ether. The polymer product was collected by filtration and dried to constant weight at 30°C under vacuum. Then, the polymerization conversion was calculated according to the weight method.

[0100] The molecular structure of the bifunctional halogen initiator in this embodiment is as follows:

[0101]

[0102] The methacrylic resins of Example 5, Example 6 and Comparative Example 1 were used for photolithography, and the mask line width used was 200 nanometers. The photolithography results are as follows: Figure 5 As shown, according to the exposure dose, the exposure sensitivity of the three resins is ranked as follows: three-arm methacrylate resin > two-arm methacrylate resin > conventional methacrylate resin (the smaller the exposure dose, the higher the exposure sensitivity).

[0103] Example 8 Preparation of two-arm methacrylic resin

[0104] A bifunctional halogen initiator (II-12) was used as an initiator for a metal or metal salt-catalyzed reversible-deactivated free radical polymerization, and the feed was added at a molar ratio of [tBMA]0 / [ADAMA]0 / [MAMA]0 / [HAMA]0 / [II-12]0 / [CuBr]0 / [PMDETA]0=15 / 15 / 15 / 15 / 1 / 3 / 5, tBMA (1.52 g, 10.7 mmol), ADMA (2.35 g, 10.7mmol), MAMA (2.50g, 10.7mmol), HAMA (2.52g, 10.7mmol), initiator II-12 (0.50g, 0.7mmol), CuBr (0.31g, 2.1mmol) and PMDETA (0.62g, 3.6mmol) were added to a 25mL reaction bottle equipped with a magnetic stirrer and dried, and 10mL of anhydrous toluene was added as a polymerization solvent. Then the reaction atmosphere was replaced with an inert gas through a double-row tube, and sealed and placed in a magnetic stirrer at 90°C, and the polymerization reaction was set for 24h. After the polymerization reaction was completed, the reaction mixture was taken out and diluted with 20mL tetrahydrofuran and precipitated with 500mL petroleum ether. The polymer product was collected by filtration and dried to constant weight at 30°C under vacuum. Then, the polymerization conversion was calculated according to the weight method.

[0105] The molecular structure of the two-arm methacrylic resin in this embodiment is as follows:

[0106]

[0107] Example 9 Preparation of three-arm methacrylic resin

[0108] A trifunctional halogen initiator (II-13) was used as an initiator for a metal or metal salt-catalyzed reversible-deactivated free radical polymerization, and the feed was added at a molar ratio of [tBMA]0 / [ADAMA]0 / [MAMA]0 / [HAMA]0 / [I-13]0 / [CuBr]0 / [PMDETA]0=15 / 15 / 15 / 15 / 1 / 4 / 6, tBMA (1.87 g, 10.3 mmol), ADAMA (2.28 g, 10.3mmol), MAMA (2.42g, 10.3mmol), HAMA (2.44g, 10.3mmol), initiator II-13 (0.70g, 0.69mmol), CuBr (0.39g, 2.74mmol) and PMDETA (0.72g, 4.12mmol) were added to a 25mL reaction bottle dried with a magnetic stirrer, and 10mL of toluene was added as the polymerization solvent. Then the reaction atmosphere was replaced with an inert gas through a double-row tube, and after sealing, it was placed in a magnetic stirrer at 90 degrees, and the polymerization reaction was set for 24h. After the polymerization reaction was completed, the reaction mixture was taken out and precipitated using 500mL of petroleum ether. The polymer product was collected by filtration and dried to constant weight at 30°C under vacuum. Then, the polymerization conversion was calculated according to the weight method.

[0109] The molecular structure of the three-arm methacrylic resin in this embodiment is as follows:

[0110]

[0111] Example 10 Preparation of four-arm methacrylic resin

[0112] A tetrafunctional halogen initiator (II-22) was used as an initiator for a metal or metal salt-catalyzed reversible-deactivated free radical polymerization, and the feed was added at a molar ratio of [tBMA]0 / [ADAMA]0 / [MAMA]0 / [HAMA]0 / [II-22]0 / [CuBr]0 / [PMDETA]0=15 / 15 / 15 / 15 / 1 / 5 / 6, tBMA (100.0 mg, 0.70 mmol), ADAMA (154.9 m g, 0.70mmol), MAMA (164.8mg, 0.70mmol), HAMA (166.2mg, 0.70mmol), initiator II-22 (56.2mg, 0.04mmol), CuBr (33.6mg, 0.24mmol) and PMDETA (48.6mg, 0.28mmol) were added to a 5mL reaction bottle dried with a magnetic stirrer, and 2mL of toluene was added as the polymerization solvent. Then the reaction atmosphere was replaced with an inert gas through a double-row tube, and the mixture was sealed and placed in a magnetic stirrer at 90°C for a set polymerization time. After the polymerization reaction was completed, the reaction mixture was taken out and precipitated using 200mL of petroleum ether. The polymer product was collected by filtration and dried to constant weight at 30°C under vacuum. Then, the polymerization conversion was calculated according to the weight method.

[0113] The molecular structure of the four-arm methacrylic resin in this embodiment is as follows:

[0114]

[0115] The synthesis data of the methacrylic acid resin in the above-mentioned Examples 5 to 10 and Comparative Example 1 are shown in the following table.

[0116]

[0117] Note: The yield was calculated by weighing method; Mn and PDI were obtained by GPC test.

[0118] It can be seen from the above table that the yield of the methacrylic resin prepared by the present invention is greater than 50%, and polymer structures with different monomer ratios and different molecular weights can be designed. The number average molecular weight obtained by testing is greater than 5000 g / mol, and the molecular weight distribution is relatively narrow, ranging from 1.20 to 1.50.

[0119] In the present invention, the polymerization monomers used may also be other (meth)acrylate monomers other than those in the above examples for homopolymerization or copolymerization, and the same results and conclusions may be obtained by using the same or similar polymerization methods.

[0120] In summary, the present invention provides a method for preparing a methacrylate polymer having an acetal structure in the main chain. The invention introduces a class of halogen-containing compounds as free radical polymerization initiators, and utilizes a reversible-inactivation free radical polymerization method catalyzed by metal or metal salt to prepare a (meth)acrylic resin having an acetal group in the main chain. The molecular weight of the resin is controllable and the molecular weight distribution is relatively narrow (Mw / Mn<1.50), which meets the characteristics of "active" free radical polymerization.

[0121] The present invention provides an application of a (meth) acrylic resin containing an acetal group in the main chain of the above technical solution in the field of photoresist.

[0122] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the technical principles of the present invention, and these improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. An acrylic resin polymer, characterized in that It has a structure as shown in formula (I): wherein x=1-1600; R1 is selected from the residue of a diol or a dihydric phenol, the residue of a triol or a trihydric phenol, the residue of a tetraol or a tetrahydric phenol, and n≥2; R2 is selected from the residue of a diol or a dihydric phenol; R3 is selected from a methyl group or a hydrogen atom; R4 is selected from a halogen bromine atom or a chlorine atom; R5 is selected from any one of a benzyl group, an adamantyl group or a hydroxy-substituted adamantyl group, a C1-C12 alkyl group or a hydroxy-substituted C1-C12 alkyl group, and a glycidyl group; The molecular weight of the acrylic resin polymer is 1000 to 200000 g / mol, and the molecular weight distribution is 1.04 to 2.50; Preferably, R1 is selected from the residue of a dihydric alcohol or a dihydric phenol, and n is 2, or, R1 is selected from the residue of a trihydric alcohol or a trihydric phenol, and n is 3, or, R1 is selected from the residue of a tetrahydric alcohol or a tetrahydric phenol, and n is 4.

2. The method for preparing an acrylic resin polymer according to claim 1, wherein: include: In an inert gas atmosphere, an acrylate monomer or a methacrylate monomer, a halogen initiator, a catalyst and a ligand are subjected to a metal or metal salt-catalyzed reversible-deactivated free radical polymerization reaction in a solvent at 0 to 110° C. to obtain the acrylic resin polymer; Wherein, the halogen initiator has a structure as shown in formula (II): R1 is selected from the residue of a diol or a dihydric phenol, the residue of a triol or a trihydric phenol, the residue of a tetraol or a tetrahydric phenol, and n≥2; R2 is selected from the residue of a diol or a dihydric phenol; R3 is selected from a methyl group or a hydrogen atom; R4 is selected from a halogen bromine atom or a chlorine atom; Preferably, R1 is selected from the residue of a dihydric alcohol or a dihydric phenol, and n is 2, or, R1 is selected from the residue of a trihydric alcohol or a trihydric phenol, and n is 3, or, R1 is selected from the residue of a tetrahydric alcohol or a tetrahydric phenol, and n is 4.

3. The preparation method according to claim 2, characterized in that: The molar ratio of the acrylic acid ester monomer or the methacrylic acid ester monomer, the halogen initiator, the catalyst and the coordination agent is (1-1600):1:(0.05-10):(0.15-15).

4. The preparation method according to claim 2 or 3, characterized in that: The acrylic acid ester monomer or methacrylic acid ester monomer is selected from any one or more combinations of benzyl methacrylate, methyl methacrylate, tert-butyl methacrylate, glycidyl methacrylate, n-butyl methacrylate, dicyclopentyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, 2-methyl-2-adamantyl methacrylate, 2-ethyl-2-adamantyl methacrylate, 1-adamantyl methacrylate, 3-hydroxy-1-adamantyl methacrylate, benzyl acrylate, methyl acrylate, tert-butyl acrylate, glycidyl acrylate, n-butyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, 2-methyl-2-adamantyl acrylate, 2-ethyl-2-adamantyl acrylate, 1-adamantyl acrylate, and 3-hydroxy-1-adamantyl acrylate.

5. The preparation method according to claim 2 or 3, characterized in that: The diol or dihydric phenol is selected from the structures shown in any one or more of the following formulae: And / or, the trihydric alcohol or trihydric phenol is selected from the structures shown in any one or more of the following formulae: And / or, the tetrahydric alcohol or tetrahydric phenol is selected from the structures shown in any one or more of the following formulae:

6. The preparation method according to claim 5, characterized in that: The halogen initiator is selected from one or more of the compounds represented by formula II-1 to formula II-24:

7. The preparation method according to claim 2 or 3, characterized in that: The catalyst includes any one of copper, iron, cupric chloride, cuprous chloride, ferric bromide, ferrous bromide, cupric bromide, and cuprous bromide, or a combination of two or more thereof.

8. The preparation method according to claim 2 or 3, characterized in that: The complexing agent includes any one of N,N,N′,N,′N″-pentamethyldiethylenetriamine, 2,2′-bipyridine, and 1,1,4,7,10,10-hexamethyltriethylenetetramine, or a combination of two or more thereof.

9. The preparation method according to claim 2 or 3, characterized in that: The solvent includes any one of toluene, xylene, tetrahydrofuran, dioxane, and ethyl acetate, or a combination of two or more thereof.

10. Use of the acrylic resin polymer according to claim 1 in preparing photoresist.

Citation Information

Patent Citations

  • Oil soluble polymers

    CN101189268A

  • Photoresist resin monomer synthesized from carboxylic acid compound and synthesis method thereof

    CN111100007A

  • Photosensitive film-forming resin, photoresist composition and preparation method of photoresist composition

    CN113717314A

  • Polymer, production method thereof, and optical material

    JP2018154669A