Bottom anti-reflection film resin and composition, preparation method of bottom anti-reflection film resin and composition, and pattern forming method
By using monomer I, monomer II and monomer III in the photoresist for radical polymerization, the problem of poor hole filling effect of the bottom anti-reflective coating in the prior art is solved, and the problem of achieving the effect of the hole filling of the bottom anti-reflective coating in the existing technology is achieved. High refractive index and good hole filling effect improve the resolution of photoresist images.
Patent Information
- Application Number
- CN202411179981.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
The existing bottom anti-reflective coatings are poorly effective in filling the structural defects of the substrate surface, resulting in reflected and refracted light interference, affecting the resolution and uniformity of the photoresist image.
The polymerization reaction is carried out under a radical initiator by monomer I, monomer II and monomer III to form a bottom antireflective film resin with 7-oxabicyclic[2.2.1]heptane, acid anhydride and thiol structures, and by Self-crosslinking reaction improves refractive index and hole filling effect.
The refractive index and hole filling ability of the bottom anti-reflective film coating are significantly improved, the circular notch and swing curve effects caused by reflected light scattering are reduced, and the resolution of the photoresist image is improved.
Smart Images

Figure CN118930721A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor coating materials, and in particular relates to a bottom anti-reflection film resin and a composition, and a preparation method and a pattern forming method thereof. Background Art
[0002] Photoresist is a photosensitive film used to transfer an image to a substrate. During the photolithography process, a photoresist layer is formed on the substrate, and then the photoresist layer is exposed to an activating radiation source through a photomask. After exposure, the photoresist is developed to provide a relief image, thereby completing the photolithography. Photoresists are mainly used in semiconductor manufacturing, and their purpose is to convert highly polished semiconductor wafers (such as silicon) into a complex matrix of electronic conduction paths that can perform circuit functions. Correct photoresist processing is the key to achieving this goal. Exposure is considered to be a very critical step to obtain a high-resolution photoresist image. The reflection of the activating radiation used to expose the photoresist usually limits the resolution of the image formed in the photoresist layer. The reflection of the irradiation at the substrate / photoresist interface can form spatial variations in the irradiation intensity of the photoresist, thereby causing uneven photoresist line widths during development. Irradiation can also be scattered from the substrate / photoresist interface to the photoresist area that does not need to be exposed, thereby causing line width variations again.
[0003] At present, the method of reducing irradiation reflection is to add a bottom anti-reflection coating between the photoresist and the substrate, which can effectively eliminate the interference standing wave. The bottom anti-reflection coating can increase the exposure energy range and focal length, reduce the reflection of light, and thus improve the effect of image resolution. According to the materials currently used, the bottom anti-reflection coating can be divided into an inorganic anti-reflection coating and an organic anti-reflection coating. The organic anti-reflection coating material is made of polymer. Compared with the inorganic anti-reflection coating, the organic anti-reflection coating does not require complex and expensive equipment, and the organic anti-reflection coating has a higher light absorptivity and excellent etching rate. Although the introduction of the bottom anti-reflection coating can reduce light reflection to a certain extent, due to certain structural defects on the surface of the substrate material, the bottom anti-reflection coating cannot completely fill these defects, which will lead to the existence of gaps, thereby causing the swing curve effect and the concave effect, and the anti-reflection effect is not ideal. In addition, the increase in the refractive index of the bottom anti-reflection coating can make the reflected and refracted light interfere with each other to offset each other, thereby suppressing reflection. Therefore, increasing the refractive index of the bottom anti-reflection coating refractive index is an effective means to reduce light reflection. Summary of the invention
[0004] The first purpose of the present invention is to overcome the defects of the existing bottom anti-reflection coating, that is, the poor anti-reflection effect and poor hole-filling effect, and to provide a new method for preparing a bottom anti-reflection film resin. The bottom anti-reflection film resin prepared by this method can improve the refractive index of the bottom anti-reflection film coating and has a good hole-filling effect.
[0005] Specifically, the preparation method of the bottom anti-reflection film resin provided by the present invention comprises polymerizing monomer I, monomer II and monomer III in the presence of a free radical initiator to obtain the bottom anti-reflection film resin; the monomer I has a structure shown in formula (1), the monomer II has a structure shown in formula (2), and the monomer III has a structure shown in formula (3);
[0006]
[0007] In formula (1), W is O or S, k is 0 or 1;
[0008] In formula (2), R 1 , R 2 and R 3 Independently of each other, H or C 1 -C 5 The alkyl group, R 4 is a chromophore, X is absent or is C 1 -C 5 An alkylene, oxygen, carbon or ester group;
[0009] In formula (3), R 1 , R 2 and R 3 Independently of each other, H or C 1 -C 5 alkyl, X` is absent or is C 1 -C 5 An alkylene group, an oxygen group, a carbon group or an ester group.
[0010] The second object of the present invention is to provide a bottom anti-reflection film resin prepared by the above method.
[0011] The third object of the present invention is to provide a bottom anti-reflection film composition, which contains the above-mentioned bottom anti-reflection film resin, an acid generator, an organic solvent and an optional surfactant.
[0012] The fourth object of the present invention is to provide a method for preparing the above anti-reflection coating composition, which comprises uniformly mixing a bottom anti-reflection film resin, an acid generator, an organic solvent and an optional surfactant.
[0013] A fifth object of the present invention is to provide a pattern forming method, the method comprising:
[0014] Applying the anti-reflective coating composition onto a substrate and thermally curing the composition to form an anti-reflective coating on the substrate;
[0015] forming a photoresist layer on the anti-reflective coating;
[0016] The photoresist layer is exposed and developed to form a photoresist pattern.
[0017] The key to the present invention is to subject monomers I, II and III with specific structures to free radical polymerization reaction, wherein monomer I simultaneously has a tightly bonded 7-oxabicyclo[2.2.1]heptane structure and anhydride structure and the anhydride is located at the end, monomer II is an acrylic ester compound with a chromophore, and monomer III is an acrylic ester compound with a mercapto group. After free radical polymerization reaction, these three monomers can bond 7-oxabicyclo[2.2.1]heptane structure, anhydride structure, acrylic ester structure with a chromophore and acrylic ester structure with a mercapto group on the same polymer chain, the anhydride structure derived from monomer I and the mercapto group derived from monomer III are suspended on both sides of the polymer main chain, and these two groups can cause the polymer to undergo a self-crosslinking reaction, so that the bottom anti-reflection film resin obtained can be well filled into the surface of the substrate, thereby giving it a high refractive index and a good hole-filling effect. Accordingly, when the bottom anti-reflective film resin is applied to photolithography, it can reduce the circular notch caused by scattering of reflected light, alleviate the swing curve effect and concave notch effect caused by different photoresist thickness due to the substrate surface morphology, and ultimately achieve the effect of improving image resolution. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a scanning electron microscope image (SEM image) of a cross section of a bottom anti-reflective coating formed on a silicon substrate using the anti-reflective coating composition obtained in Example 1;
[0019] Figure 2 is a SEM image of a cross section of a bottom anti-reflective coating formed on a silicon substrate using the anti-reflective coating composition obtained in Example 2;
[0020] Figure 3 is a SEM image of a cross section of a bottom anti-reflective coating formed on a silicon substrate using the anti-reflective coating composition obtained in Example 3;
[0021] Figure 4 This is a SEM image of a cross section of the anti-reflective coating composition obtained in Comparative Example 1 after forming a bottom anti-reflective coating on a silicon substrate;
[0022] Figure 5 This is a SEM image of the cross section of a bottom anti-reflective coating formed on a silicon substrate using the anti-reflective coating composition obtained in Comparative Example 2. DETAILED DESCRIPTION
[0023] The preparation method of the bottom anti-reflection film resin provided by the present invention comprises polymerizing monomer I, monomer II and monomer III in the presence of a free radical initiator. In the preparation process of the bottom anti-reflection film resin, as long as the three monomers are subjected to free radical polymerization at the same time, the ratio between the three monomers is not particularly limited, but in order to make it have a higher refractive index and a better hole filling effect, preferably, the molar ratio of the monomer I, monomer II and monomer III is (1-5):1:(1-5). Specifically, based on the content of monomer II as 1 mol, the content of the monomer I and monomer III is preferably independently 1-5 mol, such as 1 mol, 1.5 mol, 2 mol, 2.5 mol, 3 mol, 3.5 mol, 4 mol, 4.5 mol, 5 mol or any value therebetween.
[0024] In the present invention, the monomer I has a structure represented by formula (1), and specifically may have at least one of the structures represented by formula (1-1) to formula (1-3).
[0025]
[0026] In formula (1), W is O or S, and k is 0 or 1.
[0027] In the present invention, the monomer I can be purchased commercially or prepared according to various existing methods, which will not be described in detail here.
[0028] In the present invention, the monomer II has a structure shown in formula (2):
[0029]
[0030] In formula (2), R 1 , R 2 and R 3 Independently of each other, H or C 1 -C 5 The alkyl group is preferably H or C 1 -C 3 Alkyl; R 4 is a chromophore, preferably an aromatic hydrocarbon group having 1 to 4 single rings or condensed rings; X is absent or is C 1 -C 5 The alkylene, oxygen, carbonyl or ester group is preferably absent or C 1 -C 3 The C 1 -C 5Specific examples of the alkyl group include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl or neopentyl. The chromophore may be any existing group capable of producing an ultraviolet absorption band, specifically an aromatic hydrocarbon group having 1 to 4 single rings or condensed rings, examples of which include, but are not limited to, phenyl, o-tolyl, 1-naphthyl, 2-naphthyl or anthracenyl. The C 1 -C 5 Specific examples of the alkylene group include, but are not limited to, methylene, ethylene, n-propylene, isopropylene, n-butylene, sec-butylene, isobutylene, tert-butylene, n-pentylene, isopentylene, tert-pentylene or neopentylene. From the perspective of raw material availability, the monomer II preferably has at least one of the structures shown in formula (2-1) to formula (2-4);
[0031]
[0032] In the present invention, the monomer III has a structure shown in formula (3):
[0033]
[0034] In formula (3), R 1 , R 2 and R 3 Independently of each other, H or C 1 -C 5 The alkyl groups are preferably independently H or C 1 -C 3 alkyl; X' is absent or is C 1 -C 5 An alkylene group, oxygen group, carbon group or ester group, preferably C 1 -C 3 The C 1 -C 5 Specific examples of the alkyl group include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl or neopentyl. 1 -C 5 Specific examples of the alkylene group include, but are not limited to, methylene, ethylene, n-propylene, isopropylene, n-butylene, sec-butylene, isobutylene, tert-butylene, n-pentylene, isopentylene, tert-pentylene or neopentylene.
[0035] In the present invention, the free radical initiator can be any existing initiator that can cause monomer I, monomer II and monomer III to undergo free radical copolymerization, such as azo initiators, peroxide initiators and redox initiators. Among them, specific examples of the azo initiator include, but are not limited to: at least one of dimethyl azobisisobutyrate, azobisisobutyramidine hydrochloride, azodicarbonamide, azobisisopropylimidazoline hydrochloride, azoisobutylcyanoformamide, azobiscyclohexylcarbonitrile, azobiscyanovaleric acid, azobisisopropylimidazoline, azobisisobutyronitrile, azobisisovaleronitrile and azobisisoheptylonitrile. Specific examples of the peroxide initiator include, but are not limited to: at least one of hydrogen peroxide, ammonium persulfate, sodium persulfate, potassium persulfate, benzoyl peroxide and tert-butyl benzoyl peroxide. Specific examples of the redox initiator include, but are not limited to: at least one of sulfate-sulfite, persulfate-thiourea, persulfate-organic salt and ammonium persulfate-fatty amine. Wherein, the sulfate-sulfite can be selected from at least one of sodium sulfate-sodium sulfite, potassium sulfate-potassium sulfite, and ammonium sulfate-ammonium sulfite; the persulfate-thiourea can be selected from at least one of sodium persulfate-thiourea, potassium persulfate-thiourea, and ammonium persulfate-thiourea; the persulfate-organic salt can be selected from at least one of sodium persulfate-potassium acetate, potassium persulfate-potassium acetate, and ammonium persulfate-ammonium acetate; the ammonium persulfate-fatty amine can be selected from at least one of ammonium persulfate-N,N-tetramethylethylenediamine and ammonium persulfate-diethylamine. In addition, the present invention has no particular restriction on the amount of the free radical initiator, but in order to take into account the initiation rate and the molecular weight of the polymer product, the amount of the free radical initiator is preferably 0.01-0.1% of the total weight of the monomer, and more preferably 0.01-0.08%.
[0036] In the present invention, the conditions of the polymerization reaction preferably include a temperature of 80 to 120°C, such as 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C or any value therebetween; a time of 5 to 20 hours, such as 5h, 8h, 10h, 12h, 15h, 18h, 20h or any value therebetween. In addition, the polymerization reaction is generally carried out under the protection of an inert gas in order to overcome oxygen inhibition and allow the polymerization reaction to proceed smoothly. The inert gas refers to any gas or gas mixture that does not chemically react with the reactants and products, such as one or more of nitrogen, helium and the zero group gases of the periodic table.
[0037] The invention also provides a bottom anti-reflection film resin prepared by the method.
[0038] In the present invention, the weight average molecular weight Mw of the bottom anti-reflection film resin is preferably 1000-100000 Dalton, such as 1000, 5000, 10000, 20000, 30000, 40000, 50000, 60000, 70000, 80000, 90000, 100000 or any value therebetween; the dispersion degree PDI is preferably 1.2-2.5, such as 1.2, 1.4, 1.6, 1.8, 2, 2.2, 2.4, 2.5 or any value therebetween.
[0039] The bottom anti-reflection film composition provided by the present invention contains the bottom anti-reflection film resin, an acid generator, an organic solvent and an optional surfactant.
[0040] In the present invention, based on the total weight of the bottom anti-reflection film composition, the content of the bottom anti-reflection film resin is preferably 8-20wt%, such as 8wt%, 10wt%, 12wt%, 15wt%, 18wt%, 20wt% or any value therebetween; the content of the acid generator is preferably 0.01-5wt%, such as 0.01wt%, 0.1wt%, 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt% or any value therebetween; the content of the organic solvent is preferably 70-90wt%, such as 70wt%, 75wt%, 80wt%, 85wt%, 90wt% or any value therebetween; the content of the surfactant is preferably 0-5wt%, such as 0, 0.5wt%, 1wt%, 2wt%, 4wt%, 5wt% or any value therebetween.
[0041] In the present invention, the acid generator mainly plays the role of promoting the cross-linking reaction of the bottom anti-reflection film resin. The acid generator can use a conventional photoacid generator (PAG) and / or a thermal acid generator (thermal acid generator), and can be specifically selected from at least one of a sulfonium salt-based compound, an iodine salt-based compound, a salt-based compound, an organic sulfonic acid, etc. Specific examples of the acid generator include, but are not limited to, dodecylbenzenesulfonic acid, p-toluenesulfonic acid, phthalimido trifluoromethanesulfonate, phthalimido trifluoromethanesulfonate, dinitrobenzyl toluenesulfonate, dinitrobenzyl toluenesulfonate, n-decyl disulfone, naphthyl imino trifluoromethanesulfonate, naphthyl imino trifluoromethanesulfonate, diphenyl iodine trifluoromethanesulfonate, diphenyl iodine perfluorobutyl sulfonate, diphenyl iodine hexafluorophosphate, diphenyl iodine hexafluoroarsenate, diphenyl iodine hexafluoroantimonate, diphenyl p-methoxyphenyl sulfonium trifluoromethanesulfonate, diphenyl p-toluenesulfonium trifluoromethanesulfonate, diphenyl At least one of p-tert-butylphenylsulfonium trifluoromethanesulfonate, diphenyl-p-isobutylphenylsulfonium trifluoromethanesulfonate, triphenylsulfonium trifluoromethanesulfonate, tri(p-tert-butylphenyl)sulfonium trifluoromethanesulfonate, diphenyl-p-methoxyphenylsulfonium perfluorobutylsulfonate, diphenyl-p-tolylsulfonium perfluorobutylsulfonate, diphenyl-p-tert-butylphenylsulfonium perfluorobutylsulfonate, diphenyl-p-isobutylphenylsulfonium perfluorobutylsulfonate, triphenylsulfonium perfluorobutylsulfonate, tri-p-tert-butylphenylsulfonium perfluorobutylsulfonate, hexafluoroarsenate, hexafluoroarsenate, triphenylsulfonium hexafluoroantimonate and dibutylnaphthylsulfonium trifluoromethanesulfonate.
[0042] In the present invention, the organic solvent can be various existing inert liquid media, and specific examples thereof include but are not limited to: one or more of propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, cyclohexanone, cyclopentanone, butyrolactone, N-methylpyrrolidone, and propylene glycol n-propyl ether.
[0043] In the present invention, the surfactant may be a fluorinated surfactant and / or a non-fluorinated surfactant, preferably a non-ionic fluorinated surfactant. Wherein, the non-ionic fluorinated surfactant may be a perfluorinated C4 surfactant (such as FC-4430 and FC-4432 surfactants from 3M Corporation), a fluorodiol (such as POLYFOX PF-636, PF-6320, PF-656 and PF-6520 fluorosurfactants from Omnova).
[0044] In addition, the bottom anti-reflection film composition provided by the present invention does not need to provide an additional crosslinking agent because the bottom anti-reflection film resin itself can be self-crosslinked.
[0045] The preparation method of the anti-reflective coating composition provided by the present invention comprises uniformly mixing a bottom anti-reflective film resin, an acid generator, an organic solvent and an optional surfactant. The method and conditions for uniform mixing can be conventionally selected in the art, which is known to the art and will not be described in detail herein.
[0046] The pattern forming method provided by the present invention comprises: coating the anti-reflective coating composition on a substrate and performing thermal curing to form an anti-reflective coating on the substrate; forming a photoresist layer on the anti-reflective coating; exposing and developing the photoresist layer to form a photoresist pattern.
[0047] In the present invention, the substrate can be a silicon, silicon dioxide or aluminum-aluminum oxide microelectronic wafer, or a gallium arsenide, silicon carbide, ceramic, quartz or copper substrate. It can also be appropriately used as a substrate for liquid crystal display or other flat panel display applications, such as a glass substrate, an indium tin oxide coated substrate, etc. It can also be used as a substrate for optical and optoelectronic devices (such as waveguides).
[0048] In the present invention, before applying the photoresist composition on the anti-reflective coating composition, the anti-reflective coating composition needs to be cured to form an anti-reflective coating. The curing conditions vary with the components of the anti-reflective coating composition, and more specifically, the curing conditions depend on the acid generator used in the anti-reflective coating composition. The typical curing temperature is generally 90 to 240° C., preferably 150 to 210° C. The curing conditions preferably make the anti-reflective coating composition substantially insoluble in the photoresist solvent and developer solution used.
[0049] The present invention will be described in detail below through examples.
[0050] Preparation Example 1: Synthesis of Monomer Ⅰ
[0051]
[0052] Add 10.8 g of itaconic anhydride (100 mmol), 6.8 g of furan (100 mmol) and 100 mL of toluene to a three-necked flask equipped with magnetic stirring, nitrogen protection and reflux device, heat until the solid is completely dissolved, then continue to heat to reflux and maintain for 6 hours. The reaction solution is cooled to room temperature, a large amount of solid precipitates, filter and rinse the filter cake with a small amount of toluene, and vacuum dry to obtain 14.6 g of colorless solid product with a yield of 83%. The colorless solid is monomer I.
[0053] The solid product was subjected to nuclear magnetic resonance detection, and the results of nuclear magnetic resonance detection were as follows: 1 H-NMR (300MHz, CDCl 3)δ: 1.52 (0.5H, d), 1.98-2.06 (1H, m), 2.65 (0.5H, dd), 2.76 (1H, s), 3.12 (1H, q), 4.83 (0.5H, m), 5.09 (0.5H, m), 5.14-5.23 (1H, m), 6.33 (0.5H, dd), 6.50 (0.5H, dd), 6.63 (0.5H, dd), 6.68 (0.5H, dd) ppm. It can be seen that the solid product has the structure shown in formula (1).
[0054] Synthesis Example 1: Synthesis of Polymer A
[0055] 18g (100mmol) of monomer I, 27.63g (100mmol) of 9-anthracenemethyl methacrylate, 7.41g (100mmol) of 2-propylene-1-thiol and 53g of propylene glycol monomethyl ether acetate were added to the reaction container, and stirred for 60min under nitrogen until the solid was completely dissolved, then the temperature was raised to 90°C and 1.0g of azobisisoheptanenitrile was added, and the reaction was stirred for 12h under a nitrogen atmosphere at 90°C to obtain a self-crosslinking polymer solution. The self-crosslinking polymer solution was precipitated in isopropanol and filtered, and the filter cake was placed in a 50°C vacuum drying oven and dried for 12h to obtain a bottom anti-reflection film resin, namely polymer A. The weight average molecular weight of the bottom anti-reflection film resin is 12040, and the dispersion coefficient is 1.3.
[0056] Synthesis Example 2: Synthesis of Polymer B
[0057] 36g (200mmol) of monomer I, 27.63g (100mmol) of 9-anthracenemethyl methacrylate, 51.1g (500mmol) of 3-methyl-2-butene-1-thiol and 55.85g of propylene glycol monomethyl ether acetate were added to the reaction container, and stirred for 60min until completely dissolved under nitrogen, then the temperature was raised to 90°C and 1.0g of azobisisoheptanenitrile was added, and the reaction was stirred for 20h under nitrogen atmosphere at 80°C to obtain a self-crosslinking polymer solution. The self-crosslinking polymer solution was precipitated in isopropanol and filtered, and the filter cake was placed in a 50°C vacuum drying oven and dried for 12h to obtain a bottom anti-reflection film resin, which is polymer B. The weight average molecular weight of the bottom anti-reflection film resin is 15355, and the dispersion coefficient is 1.7.
[0058] Synthesis Example 3: Synthesis of Polymer C
[0059] 90g (500mmol) of monomer I, 15.42g (100mmol) of 1-vinyl naphthyl ester, 14.82g (200mmol) of 2-propylene-1-thiol and 40.83g of propylene glycol monomethyl ether acetate were added to the reaction container, and stirred for 60min until completely dissolved under nitrogen, then the temperature was raised to 90°C and 1.0g of azobisisoheptanenitrile was added, and the reaction was stirred for 5h under a nitrogen atmosphere of 120°C to obtain a self-crosslinking polymer solution. The self-crosslinking polymer solution was precipitated in isopropanol and filtered, and the filter cake was placed in a 50°C vacuum drying oven and dried for 12h to obtain a bottom anti-reflection film resin, namely polymer C. The weight average molecular weight of the bottom anti-reflection film resin is 9690, and the dispersion coefficient is 1.4.
[0060] Comparative Synthesis Example 1: Synthesis of Polymer D
[0061] 9.8 g (100 mmol) of maleic anhydride, 15.42 g (100 mmol) of 1-vinyl naphthyl ester, 13.01 g (100 mmol) of 2-hydroxyethyl methacrylate and 53 g of propylene glycol monomethyl ether acetate were added to the reaction container, stirred for 60 min under nitrogen gas flow until completely dissolved, then heated to 90° C. and added with 1.0 g of azobisisoheptanenitrile, stirred and reacted for 12 h under nitrogen gas atmosphere at 90° C. to obtain a self-crosslinking polymer solution. The self-crosslinking polymer solution was precipitated in isopropanol and filtered, and the filter cake was placed in a 50° C. vacuum drying oven and dried for 12 h to obtain a bottom anti-reflection film resin, namely polymer D. The weight average molecular weight of the bottom anti-reflection film resin was 12210, and the dispersion coefficient was 2.0.
[0062] Comparative Synthesis Example 2: Synthesis of Polymer E
[0063] 9.8 g (100 mmol) of maleic anhydride, 27.63 g (100 mmol) of 9-anthracenemethyl methacrylate, 7.41 g (100 mmol) of 2-propylene-1-thiol and 53 g of propylene glycol monomethyl ether acetate were added to the reaction container, stirred for 60 min under nitrogen gas flow until completely dissolved, then heated to 90° C. and added with 1.0 g of azobisisoheptanenitrile, stirred and reacted for 12 h under nitrogen gas atmosphere at 90° C. to obtain a self-crosslinking polymer solution. The self-crosslinking polymer solution was precipitated in isopropanol and filtered, and the filter cake was placed in a 50° C. vacuum drying oven and dried for 12 h to obtain a bottom anti-reflection film resin, namely polymer E. The weight average molecular weight of the bottom anti-reflection film resin was 12050, and the dispersion coefficient was 1.3.
[0064] Example 1: Preparation of bottom anti-reflective coating
[0065] 10 g of polymer A, 50 g of propylene glycol monomethyl ether acetate, 50 g of ethyl lactate, and 1 g of acid generator p-toluenesulfonic acid were added to a clean bottle, shaken until all components were completely dissolved, and then filtered through a polyethylene microfilter with a pore size of 0.01 μm to obtain a bottom anti-reflective coating composition.
[0066] Example 2: Preparation of bottom anti-reflective coating
[0067] The bottom anti-reflection coating was prepared according to the method of Example 1, except that the polymer A was replaced by the same weight portion of the polymer B. The other conditions were the same as those of Example 1, to obtain a bottom anti-reflection coating composition.
[0068] Example 3: Preparation of bottom anti-reflective coating
[0069] The bottom anti-reflection coating was prepared according to the method of Example 1, except that the polymer A was replaced by the same weight portion of the polymer C. The other conditions were the same as those of Example 1 to obtain a bottom anti-reflection coating composition.
[0070] Comparative Example 1: Preparation of bottom anti-reflective coating
[0071] The bottom anti-reflection coating was prepared according to the method of Example 1, except that the polymer A was replaced by the same weight portion of the polymer D. The other conditions were the same as those of Example 1, to obtain a bottom anti-reflection coating composition.
[0072] Comparative Example 2: Preparation of bottom anti-reflective coating
[0073] The bottom anti-reflection coating was prepared according to the method of Example 1, except that the polymer A was replaced by the same weight portion of the polymer E. The other conditions were the same as those of Example 1 to obtain a bottom anti-reflection coating composition.
[0074] Test Case
[0075] The bottom anti-reflection coating compositions obtained in the above embodiments and comparative examples were spin-coated onto the etched silicon substrate, and the silicon substrate coated with the bottom anti-reflection coating composition was baked at 220° C. for 60 seconds to form a bottom anti-reflection coating with a thickness of 145 nm on the silicon substrate. The refractive index, absorbance and hole filling performance of the bottom anti-reflection coating were measured by the following method.
[0076] (1) Refractive index n: The refractive index n of the anti-reflection coating was measured at 193 nm using an ellipsometer (purchased from Woollman). The test results are shown in Table 1.
[0077] (2) Absorbance k: The absorbance k of the anti-reflection coating was tested at 193 nm using an etching device TE-8500P (purchased from TEL). The test results are shown in Table 1.
[0078] Table 1
[0079] serial number Refractive index (n) Absorbance (k) Example 1 1.94 0.28 Example 2 1.93 0.27 Example 3 1.91 0.29 Comparative Example 1 1.82 0.25 Comparative Example 2 1.86 0.24
[0080] (3) Hole filling performance: The hole filling performance of the silicon substrates of the samples obtained in the above embodiments and comparative examples was tested using a scanning electron microscope. The test results of Examples 1 to 3 and Comparative Examples 1-2 are shown in FIG. Figure 1-Figure 5 .from Figure 1-Figure 3 It can be seen that the bottom anti-reflective coating composition provided by the present invention can be well filled into the surface defects of the silicon substrate surface and has good hole-filling performance, while the bottom anti-reflective coating compositions obtained in Comparative Examples 1 and 2 cannot be well filled into the surface defects of the silicon substrate and have poor hole-filling ability.
[0081] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.
Claims
1. A method for preparing a bottom anti-reflection film resin, characterized in that: The method comprises subjecting monomer I, monomer II and monomer III to polymerization reaction in the presence of a free radical initiator to obtain the bottom anti-reflection film resin; the monomer I has a structure shown in formula (1), the monomer II has a structure shown in formula (2), and the monomer III has a structure shown in formula (3); In formula (1), W is O or S, k is 0 or 1; In formula (2), R1, R2 and R3 are independently H or a C1-C5 alkyl group, R4 is a chromophore, and X is absent or is a C1-C5 alkylene group, oxygen, carbon group or ester group; In formula (3), R 1 , R 2 and R 3 Each of them is independently H or a C1-C5 alkyl group, and X' is absent or is a C1-C5 alkylene group, oxygen, a carbon group or an ester group.
2. The method for preparing a bottom anti-reflection film resin according to claim 1, characterized in that: The molar ratio of the monomer I, the monomer II and the monomer III is (1-5):1:(1-5).
3. The method for preparing a bottom anti-reflection film resin according to claim 1, characterized in that: In formula (2), R1, R2 and R3 are independently H or C1-C3 alkyl, R4 is an aromatic hydrocarbon group having 1 to 4 single rings or condensed rings, and X is absent or is C1-C3 alkylene; in formula (3), R 1 , R 2 and R 3 are independently H or C1-C3 alkyl, and X' is C1-C3 alkylene.
4. The method for preparing a bottom anti-reflection film resin according to any one of claims 1 to 3, characterized in that: The polymerization reaction conditions include a temperature of 80 to 120° C. and a time of 5 to 20 hours.
5. A bottom anti-reflection film resin prepared by the method according to any one of claims 1 to 4.
6. The bottom anti-reflection film resin according to claim 5, characterized in that: The bottom anti-reflection film resin has a weight average molecular weight Mw of 1000 to 100000 Daltons and a dispersion degree PDI of 1.2 to 2.
5.
7. A bottom anti-reflection film composition, characterized in that: The bottom anti-reflection film composition contains the bottom anti-reflection film resin according to claim 5, an acid generator, an organic solvent, and optionally a surfactant.
8. The bottom anti-reflection film composition according to claim 7, characterized in that: Based on the total weight of the bottom anti-reflection film composition, the content of the bottom anti-reflection film resin is 8-20wt%, the content of the acid generator is 0.01-5wt%, the content of the organic solvent is 70-90wt%, and the content of the surfactant is 0-5wt%; Preferably, the acid generator is selected from dodecylbenzenesulfonic acid, p-toluenesulfonic acid, phthalimido trifluoromethanesulfonate, phthalimido trifluoromethanesulfonate, dinitrobenzyl toluenesulfonate, dinitrobenzyl toluenesulfonate, n-decyl disulfone, naphthyl imino trifluoromethanesulfonate, naphthyl imino trifluoromethanesulfonate, diphenyl iodine trifluoromethanesulfonate, diphenyl iodine perfluorobutyl sulfonate, diphenyl iodine hexafluorophosphate, diphenyl iodine hexafluoroarsenate, diphenyl iodine hexafluoroantimonate, diphenyl p-methoxyphenyl sulfonium trifluoromethanesulfonate, diphenyl p-toluenesulfonium trifluoromethanesulfonate, diphenyl p-tert-butyl at least one of diphenylsulfonium trifluoromethanesulfonate, diphenyl-p-isobutylphenylsulfonium trifluoromethanesulfonate, triphenylsulfonium trifluoromethanesulfonate, tri(p-tert-butylphenyl)sulfonium trifluoromethanesulfonate, diphenyl-p-methoxyphenylsulfonium perfluorobutylsulfonate, diphenyl-p-tolylsulfonium perfluorobutylsulfonate, diphenyl-p-tert-butylphenylsulfonium perfluorobutylsulfonate, diphenyl-p-isobutylphenylsulfonium perfluorobutylsulfonate, triphenylsulfonium perfluorobutylsulfonate, tri-p-tert-butylphenylsulfonium perfluorobutylsulfonate, hexafluoroarsenate, hexafluoroarsenate, triphenylsulfonium hexafluoroantimonate, and dibutylnaphthylsulfonium trifluoromethanesulfonate; Preferably, the organic solvent is selected from one or more of propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, cyclohexanone, cyclopentanone, butyrolactone, N-methylpyrrolidone, and propylene glycol n-propyl ether; Preferably, the surfactant is a fluorinated surfactant and / or a non-fluorinated surfactant.
9. The method for preparing the anti-reflective coating composition according to claim 7 or 8, characterized in that: The method comprises uniformly mixing a bottom anti-reflection film resin, an acid generator, an organic solvent and an optional surfactant.
10. A pattern forming method, characterized in that: The method comprises the following steps: Applying the anti-reflective coating composition according to claim 7 or 8 onto a substrate and thermally curing the substrate to form an anti-reflective coating on the substrate; forming a photoresist layer on the anti-reflective coating; The photoresist layer is exposed and developed to form a photoresist pattern.