Viscous composite phase change material with high thermal stability and preparation method and application thereof

By preparing a viscous composite phase change material with acrylate monomer and crosslinking agent with phase change components, the problem of separation of composite phase change materials under thermal stress is solved, and high thermal stability and leakage-free effect is achieved. It is suitable for Wide range of thermal management applications.

CN118930722APending Publication Date: 2024-11-12HEFEI XINNENG PHASE CHANGE NEW MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411190818.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Composite phase change materials may separate from the contact surface of the device under thermal stress or vibration, hindering heat transfer and increasing the risk of device damage, while their poor thermal stability limits high-temperature applications.

Method used

A viscous composite phase change material is prepared by radical polymerization by acrylate monomers, crosslinkers and initiators with side chains, to adjust its melting point and viscosity to ensure that the material remains viscous under external forces.

Benefits of technology

It realizes high thermal stability, leakage-free, cost-effective, and wide application range to prevent the separation of materials from the devices, ensure effective heat transfer and stable device operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930722A_ABST
    Figure CN118930722A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of thermal energy management and temperature regulation, and provides a viscous composite phase change material with high thermal stability and a preparation method and application thereof.The viscous composite phase change material is prepared through a polymerization reaction, and raw materials of the viscous composite phase change material comprise an acrylate monomer with a phase change component on a side chain, a cross-linking agent with a phase change component and an initiator. The viscous composite phase change material is prepared through a polymerization reaction, used raw materials comprise one or more of a phase change monomer with reaction activity and a cross-linking agent, the material shows good leakproof performance and thermal stability under the action of covalent cross-linking, and in addition, by adjusting the protection proportion of the phase change monomer and the cross-linking agent, the anti-leakage performance and the thermal stability of the material are improved. The enthalpy value, the melting point, the viscosity and the thermal stability of the material can be accurately adjusted, so that the obtained material has the following remarkable advantages of being adjustable in enthalpy value, melting point and viscosity, high in thermal stability, free of leakage, high in cost benefit, wide in application range and easy and convenient to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of thermal energy management and temperature regulation, and more specifically, to a viscous composite phase change material with high thermal stability and a preparation method and application thereof. Background Art

[0002] Composite phase change materials play a vital role in the field of thermal management technology due to their excellent flexibility. They can absorb or release a large amount of latent heat within a specific temperature range. Therefore, this material is widely used in thermal management technology. For example, in the heat dissipation of electronic equipment, they can absorb and store the heat generated by the equipment when it is running, and release the heat to the environment when needed, so as to maintain the stable operation of the equipment. In addition, they can also be used in building insulation, solar thermal collection systems, textile temperature regulation and many other fields;

[0003] At present, it is found in actual applications that the contact surface between the material and the device may separate due to thermal stress or vibration. This separation not only hinders the effective transfer of thermal energy, but also increases the risk of device damage due to heat accumulation.

[0004] In addition, most composite phase change materials have poor thermal stability, which limits their application in high-temperature scenarios.

[0005] In order to solve the above problems, the present application proposes a viscous composite phase change material with high thermal stability and a preparation method and application thereof. Summary of the invention

[0006] The object of the present invention is to provide a viscous composite phase change material with high thermal stability and a preparation method and application thereof, which can effectively solve the problem mentioned in the above background technology that the contact surface between the material and the device may be separated due to thermal stress or vibration. This separation not only hinders the effective transfer of thermal energy, but also increases the risk of device damage due to heat accumulation.

[0007] One of the purposes of the present invention is to provide a viscous composite phase change material with high thermal stability, which has the characteristics of adjustable melting point, adjustable viscosity, no leakage, high cost-effectiveness and wide application range.

[0008] The second object of the present invention is to provide a method for preparing the above-mentioned viscous composite phase change material, which has the effect of simple operation and can accurately adjust the melting point and viscosity of the material.

[0009] A third object of the present invention is to provide an application method of the above-mentioned viscous composite phase change material, which has the characteristic of high viscosity to prevent separation of the material from the device.

[0010] The purpose of the present invention can be achieved through the following technical solutions:

[0011] In a first aspect, the present invention provides a viscous composite phase change material with high thermal stability, wherein the raw materials of the viscous composite phase change material are composed of an acrylate monomer having a phase change component in a side chain, a crosslinking agent having a phase change component, and an initiator;

[0012] Among them, the acrylate monomer having a phase change component in the side chain includes one or more of polyethylene glycol acrylate, polyethylene glycol methacrylate, methoxypolyethylene glycol acrylate, polyethylene glycol acrylate derivatives, methyl acrylate, isooctyl methacrylate, undecyl acrylate, dodecyl acrylate, dodecyl methacrylate, tridecyl acrylate, tetradecyl acrylate, tetradecyl methacrylate, hexadecyl acrylate, octadecyl acrylate, nonadecyl acrylate, eicosyl acrylate, hexadecanyl acrylate and docosyl acrylate.

[0013] As a further optimization of the present invention, the crosslinking agent includes one or more of ethylene glycol dimethacrylate, ethylene glycol diacrylate, divinylbenzene, polyethylene glycol diacrylate, polyethylene glycol diacrylate derivatives, polyethylene glycol dimethacrylate, aziridine crosslinker, dimethylethylenediamine, tetramethylethylenediamine and dipropylene terephthalate.

[0014] As a further optimization of the present invention, the initiator is one or more of an organic peroxide initiator, an inorganic peroxide initiator, an azo initiator, a redox initiator, a photoinitiator, and the like.

[0015] As a further optimization of the present invention, the mass ratio of the monomer to the cross-linking agent is in the range of 1000:1-10:1, and the mass ratio of the monomer to the initiator is in the range of 1000:1-100:5.

[0016] In a second aspect, the present invention provides a method for preparing the above-mentioned viscous composite phase change material, the method comprising reacting a reactive phase change monomer with a crosslinking agent under the action of an initiator to generate a polymer solid-solid phase change composite material through a free radical polymerization reaction, and the specific preparation method is as follows:

[0017] S1: mixing an acrylate monomer having a phase change component on a side chain, a crosslinking agent and an initiator to form a uniform solution;

[0018] S2: solidifying the obtained mixed solution to obtain a viscous polymer solid-solid phase change composite material;

[0019] S3: The curing method includes the following two methods:

[0020] S01: placing the obtained mixed solution in a heating environment through a glass container at a temperature of 40°C-130°C, and performing a polymerization reaction under a heat preservation condition of 1-12 hours to obtain a viscous polymer solid-solid phase change composite material;

[0021] S02: Curing the obtained mixed solution under an ultraviolet curing lamp for 30-360 seconds to obtain a viscous polymer solid-solid phase change composite material.

[0022] In a third aspect, the present invention provides an application of the above-mentioned viscous composite phase change material, wherein the viscous composite phase change material is applied to the surface of an electronic device to manage and regulate the absorption and release of thermal energy thereof.

[0023] As a further optimization of the present invention, the viscous composite phase change material is also applied to textiles, and the phase change material is compounded with the matrix of the textiles and processed into textiles through spinning, weaving and knitting processes.

[0024] Wherein, the application of the viscous composite phase change material includes but is not limited to one of them.

[0025] Beneficial effects of the present invention:

[0026] The present invention provides a viscous composite phase change material, which is prepared by polymerization reaction, and the raw materials used include one or more reactive phase change monomers and cross-linking agents. Due to the effect of covalent cross-linking, the material exhibits good anti-leakage performance;

[0027] In addition, by adjusting the ratio of phase change monomer to cross-linking agent, the melting point and viscosity of the material as well as the material state can be precisely adjusted. The resulting material has the following significant advantages: adjustable melting point, adjustable viscosity, no leakage, high cost-effectiveness, wide application range and easy operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0029] Figure 1 It is a schematic diagram showing the viscosity of the experimental results of the present invention;

[0030] Figure 2 This is a schematic diagram showing the appearance of the experimental results of the present invention; DETAILED DESCRIPTION

[0031] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0032] The viscous composite phase change material with high thermal stability provided by the present application and its preparation method and application are described in detail below.

[0033] The inventor creatively proposed: by reacting a reactive phase change monomer with a cross-linking agent under the action of an initiator to generate a polymer solid-solid phase change composite material through a free radical polymerization reaction, the melting point and viscosity of the material can be accurately adjusted, and the material can have the advantages of adjustable melting point, adjustable viscosity, no leakage, high cost-effectiveness, wide application range and easy operation.

[0034] Based on this, the present application proposes a viscous composite phase change material with high thermal stability, wherein the raw materials of the viscous composite phase change material are composed of an acrylate monomer having a phase change component in the side chain, a crosslinking agent having a phase change component, and an initiator;

[0035] The acrylate monomer having a phase change component in the side chain includes at least one of polyethylene glycol acrylate, polyethylene glycol methacrylate, methoxy polyethylene glycol acrylate, polyethylene glycol acrylate derivatives, methyl acrylate, isooctyl methacrylate, undecyl acrylate, dodecyl acrylate, dodecyl methacrylate, tridecyl acrylate, tetradecyl acrylate, tetradecyl methacrylate, hexadecyl acrylate, octadecyl acrylate, nonadecyl acrylate, eicosyl acrylate, hexadecanyl acrylate and docosyl acrylate;

[0036] The crosslinking agent includes at least one of ethylene glycol dimethacrylate, ethylene glycol diacrylate, divinylbenzene, polyethylene glycol diacrylate, polyethylene glycol diacrylate derivatives, polyethylene glycol dimethacrylate, aziridine crosslinking agent, dimethylethylenediamine, tetramethylethylenediamine and dipropylene terephthalate;

[0037] The initiator is one or more of an organic peroxide initiator, an inorganic peroxide initiator, an azo initiator, a redox initiator, a photoinitiator and the like.

[0038] Among them, the mass ratio of monomer to cross-linker ranges from 1000:1 to 10:1, and the mass ratio of monomer to initiator ranges from 1000:1 to 100:5.

[0039] It should be noted that the above-mentioned viscous composite phase change material can maintain stable viscosity under the action of external force, so that the device using the material has stable performance, and cooperates with the effect of covalent cross-linking, so that the material has good anti-leakage function, thereby preventing leakage due to external force;

[0040] Correspondingly, the present invention provides a method for preparing the above-mentioned viscous composite phase change material, comprising reacting a reactive phase change monomer with a crosslinking agent under the action of an initiator to generate a polymer solid-solid phase change composite material through a free radical polymerization reaction. The specific preparation method is as follows:

[0041] S1: mixing an acrylate monomer having a phase change component on a side chain, a crosslinking agent and an initiator to form a uniform solution;

[0042] S2: solidifying the obtained mixed solution to obtain a viscous polymer solid-solid phase change composite material;

[0043] S3: The above curing method includes the following two methods:

[0044] S01: placing the obtained mixed solution in a heating environment through a glass container at a temperature of 40°C-130°C, and performing a polymerization reaction under a heat preservation condition of 1-12 hours to obtain a viscous polymer solid-solid phase change composite material;

[0045] S02: Curing the obtained mixed solution under an ultraviolet curing lamp for 30-360 seconds to obtain a viscous polymer solid-solid phase change composite material.

[0046] It should be noted that the above-mentioned curing methods include but are not limited to the above two methods. Secondly, when preparing the above-mentioned viscous composite phase change material, by adjusting the usage ratio between the acrylate monomer with phase change components and the cross-linking agent in the raw materials, the melting point, viscosity and material state of the viscous composite phase change material can be accurately controlled, and the operation is simple to improve the application range of the material.

[0047] The features and performance of the present invention are further described in detail below in conjunction with examples of different raw material usage ratios.

[0048] In the following examples and comparative examples, the preparation method of the above-mentioned viscous composite phase change material is adopted, and the parts are measured in g:

[0049] Example 1

[0050] This embodiment provides a viscous composite phase change material with high thermal stability, wherein the raw materials include 3.136 parts of lauryl acrylate, 28.224 parts of hexadecyl acrylate, 0 parts of methoxyethyl methacrylate, 0.07 parts of ethylene glycol dimethacrylate, and 0.04 parts of azobisisobutyronitrile, and after mixing, a polymerization reaction is carried out at 80° C. for 3 hours;

[0051] Example 2

[0052] This embodiment provides a viscous composite phase change material with high thermal stability, wherein the raw materials include 2.2 parts of lauryl acrylate, 13.48 parts of hexadecyl acrylate, 0 parts of methoxyethyl methacrylate, 0.02 parts of ethylene glycol dimethacrylate, and 0.04 parts of azobisisobutyronitrile, and after mixing, a polymerization reaction is carried out at 80° C. for 3 hours;

[0053] Example 3

[0054] The present embodiment provides a viscous composite phase change material with high thermal stability, wherein the raw materials include 2.2 parts of lauryl acrylate, 13.48 parts of hexadecyl acrylate, 0 parts of methoxyethyl methacrylate, 0.04 parts of ethylene glycol dimethacrylate, and 0.02 parts of azobisisobutyronitrile, and after mixing, a polymerization reaction is carried out at 80° C. for 3 hours;

[0055] Example 4

[0056] This embodiment provides a viscous composite phase change material with high thermal stability, wherein the raw materials include 2.5 parts of lauryl acrylate, 13.18 parts of hexadecyl acrylate, 0.05 parts of polymerization inhibitor, 0.04 parts of ethylene glycol dimethacrylate, and 0.02 parts of azobisisobutyronitrile, and the mixture is subjected to polymerization reaction at 80° C. for 3 hours.

[0057] Example 5

[0058] This embodiment provides a viscous composite phase change material with high thermal stability, wherein the raw materials include 2.5 parts of lauryl acrylate, 13.18 parts of hexadecyl acrylate, 0.01 parts of polymerization inhibitor, 0.04 parts of ethylene glycol dimethacrylate, and 0.02 parts of azobisisobutyronitrile, and after mixing, a polymerization reaction is carried out at 80° C. for 3 hours;

[0059] Example 6

[0060] This embodiment provides a viscous composite phase change material with high thermal stability, wherein the raw materials include 2.5 parts of lauryl acrylate, 13.18 parts of hexadecyl acrylate, 0.02 parts of polymerization inhibitor, 0.04 parts of ethylene glycol dimethacrylate, and 0.02 parts of azobisisobutyronitrile, and after mixing, a polymerization reaction is carried out at 80° C. for 3 hours;

[0061] Example 7

[0062] This embodiment provides a viscous composite phase change material with high thermal stability, wherein the raw materials include 2.5 parts of lauryl acrylate, 13.18 parts of hexadecyl acrylate, 0.04 parts of polymerization inhibitor, 0.06 parts of ethylene glycol dimethacrylate, and 0.02 parts of azobisisobutyronitrile, and after mixing, a polymerization reaction is carried out at 80° C. for 3 hours;

[0063] Example 8

[0064] This embodiment provides a viscous composite phase change material with high thermal stability, the raw materials of which include 2.5 parts of lauryl acrylate, 13.18 parts of hexadecyl acrylate, 0.04 parts of polymerization inhibitor, 0.1 parts of ethylene glycol dimethacrylate, and 0.02 parts of azobisisobutyronitrile;

[0065] Example 9

[0066] The present embodiment provides a viscous composite phase change material with high thermal stability, the raw materials of which include: 10 parts of polyethylene glycol diacrylate (Mw is 10000 g / mol) and 0.04 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone, which are mixed and then UV-cured at room temperature for 90 seconds.

[0067] Comparative Example 1

[0068] This comparative example provides a composite phase change material, wherein the raw materials include 1 part of octadecyl acrylate, 0 part of methoxyethyl methacrylate, 0 part of ethylene glycol dimethacrylate, and 0.02 part of 2-hydroxy-2-methyl-1-phenyl-1-propanone, which are mixed and then UV-cured at room temperature for 90 seconds;

[0069] Comparative Example 2

[0070] This comparative example provides a composite phase change material, wherein the raw materials include 0.8 parts of octadecyl acrylate, 0.2 parts of methoxyethyl methacrylate, 0 parts of ethylene glycol dimethacrylate, and 0.02 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone, which are mixed and then UV-cured at room temperature for 90 seconds;

[0071] Comparative Example 3

[0072] This comparative example provides a composite phase change material, wherein the raw materials include 0.8 parts of octadecyl acrylate, 0.2 parts of methoxyethyl methacrylate, 0 parts of ethylene glycol dimethacrylate, and 0.01 parts of azobisisobutyronitrile, and the raw materials are mixed and polymerized at 80°C for 3 hours;

[0073] Comparative Example 4

[0074] This comparative example provides a composite phase change material, wherein the raw materials include 0.9 parts of octadecyl acrylate, 0 parts of methoxyethyl methacrylate, 0.1 parts of ethylene glycol dimethacrylate, and 0.02 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone, which are mixed and then UV-cured at room temperature for 90 seconds;

[0075] Comparative Example 5

[0076] This comparative example provides a composite phase change material, wherein the raw materials include 1.9 parts of hexadecyl acrylate, 0 parts of methoxyethyl methacrylate, 0.1 parts of ethylene glycol dimethacrylate, and 0.02 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone, which are mixed and then UV-cured at room temperature for 90 seconds;

[0077] Comparative Example 6

[0078] This comparative example provides a composite phase change material, the raw materials of which include 1.6 parts of hexadecyl acrylate, 0 parts of methoxyethyl methacrylate, 0.4 parts of ethylene glycol dimethacrylate, and 0.02 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone, which are mixed and then UV-cured at room temperature for 90 seconds;

[0079] Comparative Example 7

[0080] This comparative example provides a composite phase change material, the raw materials of which include 7.84 parts of lauryl acrylate, 0 parts of methoxyethyl methacrylate, 0.005 parts of ethylene glycol dimethacrylate, and 0.04 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone, which are mixed and then UV-cured at room temperature for 90 seconds;

[0081] Comparative Example 8

[0082] This comparative example provides a composite phase change material, wherein the raw materials include 7.84 parts of lauryl acrylate, 0 parts of methoxyethyl methacrylate, 0 parts of ethylene glycol dimethacrylate, and 0.04 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone, which are mixed and then UV-cured at room temperature for 90 seconds;

[0083] Comparative Example 9

[0084] This comparative example provides a composite phase change material, wherein the raw materials include 2.5 parts of lauryl acrylate, 13.18 parts of hexadecyl acrylate, 0.5 parts of polymerization inhibitor, 0.04 parts of ethylene glycol dimethacrylate, and 0.02 parts of azobisisobutyronitrile, and the raw materials are mixed and subjected to polymerization reaction at 80°C for 3 hours;

[0085] Comparative Example 10

[0086] The present embodiment provides a composite phase change material, whose raw materials include 2.5 parts of lauryl acrylate, 13.18 parts of hexadecyl acrylate, 0.1 parts of polymerization inhibitor, 0.04 parts of ethylene glycol dimethacrylate, and 0.02 parts of azobisisobutyronitrile. After mixing, the material is polymerized at 80°C for 3 hours.

[0087] The viscous composite phase change materials obtained in the preparation process of the above-mentioned Examples 1-9 and Comparative Examples 1-10 at different proportions were tested using a differential scanning calorimeter DSC according to GB / T19466.3-2004 / ISO11357-3. The specific test results are shown in the following table: (The enthalpy values ​​in the following examples are obtained by testing at 260°C for ten minutes)

[0088]

[0089]

[0090]

[0091] Correspondingly, the present invention also provides an application of the above-mentioned viscous composite phase change material, where the viscous composite phase change material is applied to the surface of an electronic device to manage and regulate the absorption and release of its thermal energy.

[0092] Viscous composite phase change materials are also used in textiles. The phase change materials are compounded with the matrix of textiles and processed into textiles through spinning, weaving and knitting processes.

[0093] It should be noted that the application of the above-mentioned viscous composite phase change material includes but is not limited to the one mentioned above. By microencapsulating, coating, spinning, or mixing the phase change material with a carrier matrix, it is applied to different objects to achieve the effect of protecting the adjacent devices from strong bonding while maintaining efficient heat energy transfer.

[0094] In summary, it can be understood that the viscous composite phase change material is prepared by polymerization reaction, and the raw materials used include one or more reactive phase change monomers and cross-linking agents. By utilizing the effect of covalent cross-linking, the material exhibits good anti-leakage performance. In addition, by adjusting the ratio of phase change monomers to cross-linking agent protection, the melting point, viscosity and thermal stability of the material can be precisely adjusted, so that the resulting material has the following significant advantages: adjustable melting point, adjustable viscosity, no leakage, high thermal stability, high cost-effectiveness, wide range of applications and easy operation.

[0095] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A viscous composite phase change material with high thermal stability, characterized in that: The viscous composite phase change material is prepared by polymerization reaction, and its raw materials are composed of an acrylate monomer with a phase change component on the side chain, a crosslinking agent with a phase change component, and an initiator; Among them, the acrylate monomer having a phase change component on the side chain includes at least one of polyethylene glycol acrylate, polyethylene glycol methacrylate, methoxypolyethylene glycol acrylate, polyethylene glycol acrylate derivatives, methyl acrylate, isooctyl methacrylate, undecyl acrylate, dodecyl acrylate, dodecyl methacrylate, tridecyl acrylate, tetradecyl acrylate, tetradecyl methacrylate, hexadecyl acrylate, octadecyl acrylate, nonadecyl acrylate, eicosyl acrylate, hexadecanyl acrylate and hexadecanyl acrylate.

2. A viscous composite phase change material with high thermal stability according to claim 1, characterized in that: The crosslinking agent includes at least one of ethylene glycol dimethacrylate, ethylene glycol diacrylate, divinylbenzene, polyethylene glycol diacrylate, polyethylene glycol diacrylate derivatives, polyethylene glycol dimethacrylate, aziridine crosslinking agent, dimethylethylenediamine, tetramethylethylenediamine and propylene terephthalate.

3. The viscous composite phase change material with high thermal stability according to claim 1, characterized in that: The initiator is at least one of an organic peroxide initiator, an inorganic peroxide initiator, an azo initiator, a redox initiator, and a photoinitiator.

4. The viscous composite phase change material with high thermal stability according to claim 1, characterized in that: The mass ratio of the monomer to the cross-linking agent is in the range of 1000:1-10:1, and the mass ratio of the monomer to the initiator is in the range of 1000:1-100:

5.

5. A method for preparing a viscous composite phase change material with high thermal stability as claimed in any one of claims 1 to 4, characterized in that: The method comprises reacting a reactive phase change monomer with a crosslinking agent under the action of an initiator to generate a polymer solid-solid phase change composite material through a free radical polymerization reaction. The specific preparation method is as follows: S1: mixing an acrylate monomer having a phase change component on a side chain, a crosslinking agent and an initiator to form a uniform solution; S2: solidifying the obtained mixed solution to obtain a viscous polymer solid-solid phase change composite material.

6. The method for preparing a viscous composite phase change material with high thermal stability according to claim 5, characterized in that: The curing method includes the following two methods: S01: placing the obtained mixed solution in a heating environment through a glass container at a temperature of 40°C-130°C, and performing a polymerization reaction under a heat preservation condition of 1-12 hours to obtain a viscous polymer solid-solid phase change composite material; S02: Curing the obtained mixed solution under an ultraviolet curing lamp for 30-360 seconds to obtain a viscous polymer solid-solid phase change composite material.

7. An application of a viscous composite phase change material with high thermal stability as claimed in any one of claims 1 to 4, characterized in that: The viscous composite phase change material is applied to the surface of electronic devices to manage and regulate the absorption and release of thermal energy thereof.

8. The viscous composite phase change material with high thermal stability and its preparation method and application according to claim 7, characterized in that: The viscous composite phase change material is also applied to textiles, where the phase change material is compounded with the matrix of the textiles and processed into textiles through spinning, weaving and knitting processes.

Citation Information

Cited By

  • Phase change composite material as well as preparation method and application thereof

    CN119144158A