Filtrate reducer for oil-based drilling fluid and preparation method of filtrate reducer

By copolymerizing polymers and inorganic materials, modifying humic acid amides, the oil-based drilling fluid filtration loss loss agent is solved, and the performance of oil-based drilling fluid filtration loss agents under high temperature conditions in the prior art is solved. , achieving good temperature resistance and filter loss reduction effect.

CN118930723APending Publication Date: 2024-11-12BEIJING FAREAST LIAN CHUANG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411238139.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing oil-based drilling fluid filter reduction agents are difficult to degrade in the environment and their performance needs to be improved, especially in the presence of insufficient temperature resistance under high temperature conditions.

Method used

Using raw materials such as polyvinylpyrrolidone, styrene, vinyl amide, unsaturated esters and crosslinking agents, oil-based drilling fluid filtration loss agent is prepared through the action of initiators, and inorganic materials such as carbon microspheres and concave and convex rods are introduced. The amidation reaction modifies humic acid to form copolymers to improve temperature resistance and reduce filtration loss.

Benefits of technology

It improves the temperature resistance and filtration loss reduction effect of oil-based drilling fluid, reduces filtration loss, and solves the problem of environmental pollution. It has simple preparation method, low production cost and strong adaptability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a filtrate reducer for an oil-based drilling fluid and a preparation method of the filtrate reducer. The preparation method of the filtrate reducer for the oil-based drilling fluid comprises the following steps: adding polyvinylpyrrolidone into a mixed solvent, introducing nitrogen, and stirring at room temperature; and adding styrene, vinyl amide, unsaturated ester and a cross-linking agent, uniformly stirring, adding an initiator, carrying out a heating reaction, and after the reaction is finished, centrifuging, washing and drying to obtain the filtrate reducer for the oil-based drilling fluid. Compared with the prior art, the filtrate reducer for the oil-based drilling fluid provided by the invention has the advantages that the preparation method is simple, the temperature resistance of the filtrate reducer in the oil-based drilling fluid is improved, and the filtrate reducer can play a good role in reducing filtrate loss in the oil-based drilling fluid. The filtrate reducer for the oil-based drilling fluid is low in production cost, simple in preparation method and process, easy to implement and popularize and wide in application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil and natural gas drilling, and in particular to a fluid loss reducer for oil-based drilling fluid and a preparation method thereof. Background Art

[0002] As oil and gas exploration and development continue to develop into deep formations, drilling technology is also constantly improving. Drilling fluid, as the blood of drilling engineering, plays a vital role in the entire drilling process. Drilling fluid has excellent properties such as carrying and suspending cuttings, cooling, lubricating drill bits, stabilizing well walls, controlling downhole pressure and transmitting water power, and is known as the "blood" of drilling. Fluid loss reducer is one of the key treatment agents in oil drilling. Its normal and stable use in complex geological reservoir environments is related to the normal development of complex oil and gas wells and the safe operation of oil field sites. It is the top priority to get rid of the external dependence on crude oil imports. The process of free water in the drilling fluid penetrating into the formation under the action of pressure difference is called filtration. Excessive filtration often brings many adverse consequences to drilling work. Therefore, it is necessary to add filtration reducer to the drilling fluid during oil extraction to improve the filtration loss of drilling fluid.

[0003] On the one hand, the filtration reducer can increase the viscosity of the drilling fluid and adsorb on the surface of bentonite particles through physical effects such as hydrogen bonds and electrostatic forces to form a dense filter cake, preventing rock cuttings and sand particles from entering the drilling fluid; on the other hand, it can seal tiny pores by absorbing water and swelling, thereby reducing the filtration loss of the drilling fluid.

[0004] CN111876139A discloses an oxidized asphalt as a fluid loss reducer for oil-based drilling fluid, which is made of the following raw materials in parts by weight: 10-12 parts of sodium hydroxide solution with a mass fraction of 40%, 16-20 parts of organic solvent, 3-5 parts of auxiliary agent, 16-20 parts of dichloromethane, 6-10 parts of butylene oxide, 40-60 parts of oxidized asphalt, 4-6 parts of dispersant, 20-25 parts of white oil and 20-25 parts of diesel. The addition of dispersant makes the oxidized asphalt in a balanced state, has good thermal stability, and enhances the effect of the fluid loss reducer. The auxiliary agent promotes the swelling of the oxidized asphalt as a fluid loss reducer for oil-based drilling fluid during use, which plays a role in reducing permeability. The oxidized asphalt as a fluid loss reducer for oil-based drilling fluid has good temperature resistance. The addition of white oil and diesel in the raw materials improves the adaptability of the oxidized asphalt as a fluid loss reducer for oil-based drilling fluid. However, asphalt is difficult to degrade in the environment and has a serious pollution problem to the environment.

[0005] CN101624516A discloses an oil-based drilling fluid fluid loss reducer and a preparation method thereof, wherein the fluid loss reducer is composed of 150-200 parts of humic acid resin and 60-80 parts of organic amine by weight, wherein the humic acid resin is a reaction product generated by potassium humate or sodium humate and protonic acid under certain reaction conditions, and the protonic acid is any one of hydrochloric acid, sulfuric acid, phosphoric acid and nitric acid. The preparation method of the oil-based drilling fluid fluid loss reducer is as follows: 150-200 parts of humic acid resin and 60-80 parts of organic amine are placed in a closed container, after nitrogen is driven for 20-30 minutes, the container is heated to 180-200°C, the reaction time is maintained for 8-10 hours, the reaction is cooled to room temperature after completion, and then the product is crushed through a 60-mesh sieve to obtain an oil-based drilling fluid fluid loss reducer product. However, its performance needs to be further improved. Summary of the invention

[0006] To achieve the above object, the present invention provides a fluid loss reducer for oil-based drilling fluid.

[0007] A method for preparing a fluid loss reducer for oil-based drilling fluid comprises the following steps:

[0008] 0.1-5 parts by weight of polyvinyl pyrrolidone is added to 100-200 parts by weight of a mixed solvent, nitrogen is introduced, and the mixture is stirred at room temperature for 30-60 minutes; then 0.1-1 parts by weight of styrene, 0.1-1 parts by weight of vinyl amide, 1-2 parts by weight of unsaturated ester, and 0.5-1.5 parts by weight of a cross-linking agent are added and stirred evenly, and then 0.05-0.1 parts by weight of an initiator is added, and the mixture is heated to 70-80° C. and reacted for 1-4 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to obtain a fluid loss reducer for oil-based drilling fluid.

[0009] The mixed solvent is a mixture of methanol and water; wherein the volume ratio of methanol to water is (5-8):(1-3).

[0010] The crosslinking agent is pentaerythritol tetraacrylate.

[0011] The vinyl amide is N-vinyl caprolactam.

[0012] The unsaturated ester is at least one of octadecyl methacrylate, isooctyl acrylate, n-butyl methacrylate, and ethyl 2-methacrylate.

[0013] The initiator is azobisisobutyronitrile.

[0014] The present invention uses styrene, vinyl amide, unsaturated ester and crosslinking agent as raw materials, and under the action of an initiator, prepares a fluid loss reducer for oil-based drilling fluid, which has good temperature resistance and improves the fluid loss reduction effect. The unsaturated ester introduced in the present invention has an ester group that increases the flexibility of the molecular structure; the introduction of N-vinyl caprolactam strengthens the rigid structure of the polymer and improves the temperature resistance; the lipophilic side chains in styrene and unsaturated ester groups are relatively large, and interact with the crosslinking agent isopentyl tetraacrylate to obtain a hyperbranched structure, which improves the temperature resistance, and the viscosity is much lower than that of linear polymers with the same molecular weight.

[0015] On the basis of the above, inorganic materials are introduced to make them participate in the copolymerization of polymers. On the one hand, the temperature resistance of the entire fluid loss reducer is improved. At the same time, the interaction between inorganic materials and organic materials can alleviate the environmental pollution caused by the large-scale use of polymers. The structure of "stretching and bridging" of attapulgite and carbon microspheres can be used to form an effective blockage in a short time to prevent further invasion of filtrate. Humic acid is modified by amidation reaction to prepare oil phase humic acid, and inorganic materials are used for treatment. During the action of the fluid loss reducer, humic acid amide can also be released, which helps the organic soil particles in the oil-based drilling fluid to maintain an alternating dispersion state and form a dense filter cake on the surface of the well wall rock, thereby reducing the filtration loss of the drilling fluid.

[0016] Further preferably, a method for preparing a fluid loss reducer for oil-based drilling fluid comprises the following steps:

[0017] 0.1-5 parts by weight of polyvinyl pyrrolidone is added to 100-200 parts by weight of a mixed solvent, nitrogen is introduced, and the mixture is stirred at room temperature for 30-60 minutes; then 0.1-1 parts by weight of styrene, 0.1-1 parts by weight of vinyl amide, 1-2 parts by weight of unsaturated ester, 1-2 parts by weight of modified inorganic material, and 0.5-1.5 parts by weight of a cross-linking agent are added and stirred evenly, and then 0.05-0.1 parts by weight of an initiator is added, and the mixture is heated to 70-80° C. and reacted for 1-4 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to obtain a fluid loss reducer for oil-based drilling fluid.

[0018] The method for preparing the modified inorganic material comprises the following steps:

[0019] Add inorganic material and silane coupling agent to 50wt% ethanol aqueous solution, mix evenly, heat to 60-80°C for reaction for 1-3h, and after the reaction, centrifuge to obtain precipitate, wash, and dry to obtain silane-modified inorganic material; wherein the mass ratio of inorganic material, silane coupling agent, and ethanol aqueous solution is 1:(0.1-0.5):(30-80);

[0020] The silane-modified inorganic material is added to ethanol and dispersed evenly, and then humic acid amide is added, and stirred at 100-300 rpm for 1-2 hours at room temperature. After the reaction is completed, the precipitate is centrifuged, washed, and dried to obtain a modified inorganic material; wherein the mass ratio of the silane-modified inorganic material, ethanol, and humic acid amide is 1:(50-80):(0.1-0.6).

[0021] The silane coupling agent is at least one of γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyltri(β-methoxyethoxy)silane and vinyltriethoxysilane.

[0022] The inorganic material is at least one of carbon microspheres and attapulgite.

[0023] Further preferably, the preparation method of the carbon microspheres is: adding a carbon source to water and mixing evenly, hydrothermally reacting at 180-200° C. for 1-3 hours, and after the reaction is completed, centrifuging to obtain a precipitate, washing, and drying to obtain carbon microspheres.

[0024] The carbon source is at least one of glucose and sisal cellulose microcrystals;

[0025] The mass volume ratio of carbon source and water is 1g:(10-15)mL.

[0026] Beneficial effects of the present invention:

[0027] 1. Compared with the prior art, the preparation method of the fluid loss reducer for oil-based drilling fluid provided by the present invention is simple, and its temperature resistance in oil-based drilling fluid is improved, and it can also play a good role in reducing fluid loss in oil-based drilling fluid.

[0028] 2. The oil-based drilling fluid fluid loss reducer prepared by the present invention has low production cost, simple preparation method and process, is easy to implement and promote, and has broad application prospects. DETAILED DESCRIPTION

[0029] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0030] Introduction of some raw materials used in the embodiments of the present invention:

[0031] The preparation method of humic acid amide in the embodiment is as follows: 100 parts by weight of humic acid is added to 20 parts by weight of toluene, mixed evenly, nitrogen is introduced, 30 parts by weight of pentaethylenehexamine is added, heated to 200°C for reaction for 3 hours, and after the reaction is completed, dried and crushed to obtain humic acid amide.

[0032] Attapulgite, item number yt-006, was purchased from Lingshou County Yuteng Mineral Products Processing Factory.

[0033] The preparation method of sisal cellulose microcrystals in the embodiment is as follows: 100 g of sisal fiber is cut into 3 mm, added to a mixed solution of 30 g of sodium sulfate, 5 wt% 100 ml of sodium hydroxide, and 500 ml of water, stirred at 100° C. for 3 hours, filtered, and the filter cake is rinsed with deionized water several times; then the filter cake is placed in 500 ml of water, 15 ml of glacial acetic acid and 13 g of sodium hypochlorite solution, heated to 85° C. and stirred for 3 hours, cooled, filtered, and dried to obtain sisal cellulose microcrystals.

[0034] Other raw materials not mentioned are common raw materials in the art. The above content is only to help illustrate the present invention and should not be construed as a strict limitation of the present invention. Those skilled in the art can directly purchase or prepare the same / similar raw materials from the market. These contents will not be repeated in the examples.

[0035] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] A method for preparing a fluid loss reducer for oil-based drilling fluid comprises the following steps:

[0038] 1 part by weight of polyvinyl pyrrolidone is added to 100 parts by weight of a mixed solvent (methanol:water ratio is 7:3 by volume), nitrogen is introduced, and the mixture is stirred at room temperature for 30 minutes; then 0.5 parts by weight of styrene, 0.3 parts by weight of N-vinyl caprolactam, 1 parts by weight of octadecyl methacrylate, and 0.5 parts by weight of isopentaerythritol are added and mixed evenly, and then 0.05 parts by weight of azobisisobutyronitrile is added, and the mixture is heated to 70°C and reacted for 4 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to obtain a fluid loss reducer for oil-based drilling fluid.

[0039] Example 2

[0040] A method for preparing a fluid loss reducer for oil-based drilling fluid comprises the following steps:

[0041] 1 part by weight of polyvinyl pyrrolidone was added to 100 parts by weight of a mixed solvent (methanol:water ratio of 7:3 by volume), nitrogen was introduced, and the mixture was stirred at room temperature for 30 minutes; then 0.5 parts by weight of styrene, 0.3 parts by weight of N-vinyl caprolactam, and 1 part by weight of octadecyl methacrylate were added and mixed evenly, and then 0.05 parts by weight of azobisisobutyronitrile was added, and the mixture was heated to 70°C and reacted for 4 hours. After the reaction was completed, the mixture was centrifuged, washed, and dried to obtain a fluid loss reducer for oil-based drilling fluid.

[0042] Example 3

[0043] A method for preparing a fluid loss reducer for oil-based drilling fluid comprises the following steps:

[0044] 1 part by weight of polyvinyl pyrrolidone is added to 100 parts by weight of a mixed solvent (methanol:water ratio of 7:3 by volume), nitrogen is introduced, and the mixture is stirred at room temperature for 30 minutes; then 0.5 parts by weight of styrene, 0.3 parts by weight of N-vinyl caprolactam, 1 parts by weight of octadecyl methacrylate, 1 parts by weight of modified inorganic material, and 0.5 parts by weight of isopentaerythritol tetraacrylate are added and mixed evenly, and then 0.05 parts by weight of azobisisobutyronitrile is added, and the mixture is heated to 70°C and reacted for 4 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to obtain a fluid loss reducer for oil-based drilling fluid.

[0045] The preparation method of the modified inorganic material comprises the following steps:

[0046] (1) adding an inorganic material and γ-methacryloxypropyltrimethoxysilane to a 50wt% ethanol aqueous solution and mixing them evenly, heating them to 70°C for reaction for 2h, and after the reaction, centrifuging, washing, and drying the precipitate to obtain a silane-modified inorganic material; wherein the mass ratio of the inorganic material, γ-methacryloxypropyltrimethoxysilane, and the ethanol aqueous solution is 1:0.3:50; and the inorganic material is prepared by mixing carbon microspheres and attapulgite in a mass ratio of 1:2;

[0047] (2) The silane-modified inorganic material is added to anhydrous ethanol and dispersed evenly, and then humic acid amide is added and stirred at 200 rpm at room temperature for 1 hour. After the reaction is completed, the precipitate is centrifuged, washed, and dried to obtain the modified inorganic material; wherein the mass ratio of the silane-modified inorganic material, anhydrous ethanol, and humic acid amide is 1:50:0.6.

[0048] The preparation method of the carbon microspheres is as follows: adding a carbon source to water and mixing evenly, hydrothermally reacting at 185°C for 2 hours, and after the reaction, centrifuging to obtain a precipitate, washing, and drying to obtain carbon microspheres; wherein the carbon source is a mixture of glucose and sisal cellulose microcrystals in a mass ratio of 1:1; the mass volume ratio of the carbon source to water is 1g:10mL.

[0049] Example 4

[0050] A method for preparing a fluid loss reducer for oil-based drilling fluid comprises the following steps:

[0051] 1 part by weight of polyvinyl pyrrolidone is added to 100 parts by weight of a mixed solvent (methanol:water ratio of 7:3 by volume), nitrogen is introduced, and the mixture is stirred at room temperature for 30 minutes; then 0.5 parts by weight of styrene, 0.3 parts by weight of N-vinyl caprolactam, 1 parts by weight of octadecyl methacrylate, 1 parts by weight of modified inorganic material, and 0.5 parts by weight of isopentaerythritol tetraacrylate are added and mixed evenly, and then 0.05 parts by weight of azobisisobutyronitrile is added, and the mixture is heated to 70°C and reacted for 4 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to obtain a fluid loss reducer for oil-based drilling fluid.

[0052] The preparation method of the modified inorganic material comprises the following steps:

[0053] (1) adding an inorganic material and γ-methacryloxypropyltrimethoxysilane to a 50 wt % ethanol aqueous solution and mixing them evenly, heating them to 70° C. for reaction for 2 h, and after the reaction is completed, centrifuging, taking out a precipitate, washing, and drying to obtain a silane-modified inorganic material; wherein the mass ratio of the inorganic material, γ-methacryloxypropyltrimethoxysilane, and the ethanol aqueous solution is 1:0.3:50; and the inorganic material is attapulgite;

[0054] (2) The silane-modified inorganic material is added to anhydrous ethanol and dispersed evenly, and then humic acid amide is added and stirred at 200 rpm at room temperature for 1 hour. After the reaction is completed, the precipitate is centrifuged, washed, and dried to obtain the modified inorganic material; wherein the mass ratio of the silane-modified inorganic material, anhydrous ethanol, and humic acid amide is 1:50:0.6.

[0055] Example 5

[0056] A method for preparing a fluid loss reducer for oil-based drilling fluid comprises the following steps:

[0057] 1 part by weight of polyvinyl pyrrolidone is added to 100 parts by weight of a mixed solvent (methanol:water ratio of 7:3 by volume), nitrogen is introduced, and the mixture is stirred at room temperature for 30 minutes; then 0.5 parts by weight of styrene, 0.3 parts by weight of N-vinyl caprolactam, 1 parts by weight of octadecyl methacrylate, 1 parts by weight of modified inorganic material, and 0.5 parts by weight of isopentaerythritol tetraacrylate are added and mixed evenly, and then 0.05 parts by weight of azobisisobutyronitrile is added, and the mixture is heated to 70°C and reacted for 4 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to obtain a fluid loss reducer for oil-based drilling fluid.

[0058] The preparation method of the modified inorganic material comprises the following steps:

[0059] (1) adding an inorganic material and γ-methacryloxypropyltrimethoxysilane to a 50wt% ethanol aqueous solution and mixing them evenly, heating them to 70°C for reaction for 2h, and after the reaction, centrifuging, washing, and drying the precipitate to obtain a silane-modified inorganic material; wherein the mass ratio of the inorganic material, γ-methacryloxypropyltrimethoxysilane, and the ethanol aqueous solution is 1:0.3:50; the inorganic material is carbon microspheres; wherein the preparation method of the carbon microspheres is the same as that of Example 3;

[0060] (2) The silane-modified inorganic material is added to anhydrous ethanol and dispersed evenly, and then humic acid amide is added and stirred at 200 rpm at room temperature for 1 hour. After the reaction is completed, the precipitate is centrifuged, washed, and dried to obtain the modified inorganic material; wherein the mass ratio of the silane-modified inorganic material, anhydrous ethanol, and humic acid amide is 1:50:0.6.

[0061] Example 6

[0062] A method for preparing a fluid loss reducer for oil-based drilling fluid comprises the following steps:

[0063] 1 part by weight of polyvinyl pyrrolidone is added to 100 parts by weight of a mixed solvent (methanol:water ratio of 7:3 by volume), nitrogen is introduced, and the mixture is stirred at room temperature for 30 minutes; then 0.5 parts by weight of styrene, 0.3 parts by weight of N-vinyl caprolactam, 1 parts by weight of octadecyl methacrylate, 1 parts by weight of modified inorganic material, and 0.5 parts by weight of isopentaerythritol tetraacrylate are added and mixed evenly, and then 0.05 parts by weight of azobisisobutyronitrile is added, and the mixture is heated to 70°C and reacted for 4 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to obtain a fluid loss reducer for oil-based drilling fluid.

[0064] The preparation method of the modified inorganic material comprises the following steps:

[0065] Add inorganic material and γ-methacryloxypropyltrimethoxysilane to 50wt% ethanol aqueous solution and mix evenly, heat to 70°C for reaction for 2h, and after the reaction, centrifuge to obtain the precipitate, wash and dry to obtain a modified inorganic material; wherein the mass ratio of the inorganic material, γ-methacryloxypropyltrimethoxysilane and ethanol aqueous solution is 1:0.3:50; the inorganic material is formed by mixing carbon microspheres and attapulgite in a mass ratio of 1:2; wherein the preparation method of the carbon microspheres is the same as that in Example 3.

[0066] Test Example 1

[0067] The samples prepared in the examples were tested. According to GB / T16783.2-2012 Field Test of Drilling Fluids in Petroleum and Natural Gas Industry Part 2: Oil-Based Drilling Fluid Standard, performance tests were performed on oil-based drilling fluids and oil-based drilling fluids to which 2% of the fluid loss reducer prepared in the examples was added.

[0068] Table 1 Performance test results

[0069] AV(mPa.s) PV(mPa.s) YP(Pa) Example 1 41 30 7 Example 2 37 29 7 Example 3 48 36 10 Example 4 46 35 9 Example 5 46 35 9 Example 6 43 32 8

[0070] In Table 1, AV is the apparent viscosity, PV is the plastic viscosity, and YP is the dynamic shear force.

[0071] The fluid loss reducer prepared by the invention has good fluid loss reducing effect and strong adaptability, and has good temperature resistance and strong adaptability.

[0072] Test Example 2

[0073] Drilling fluid: 240mL 5# white oil + 60mL 20% CaCl2 solution + 8kg primary emulsifier + 4kg auxiliary emulsifier + 8kg CaO + 8kg wetting agent + 4kg organic soil + 125kg barite + 12kg fluid loss reducer. Heat-roll for 16h at 150℃, 200℃, and 240℃, and then test the high temperature and high pressure fluid loss at 150℃ and 3.5MPa.

[0074] Table 2 Test results of high temperature and high pressure filtration loss

[0075] 150℃ / mL 200℃ / mL 240℃ / mL Example 1 4.9 8.3 10.5 Example 2 6.1 9.2 13.6 Example 3 3.4 5.7 8.2 Example 4 3.8 6.4 8.5 Example 5 3.9 6.7 8.8 Example 6 4.5 7.6 9.4

[0076] It can be seen from Table 2 that as the aging temperature increases, the high temperature and high pressure fluid loss also increases. Each embodiment has a good fluid loss reduction effect, and the aging temperature is as high as 240°C, and the high temperature and high pressure fluid loss of the drilling fluid can still be controlled to be less than 15mL. Therefore, the fluid loss reducer for oil-based drilling fluid prepared by the present invention has high temperature resistance, and at the same time, the product is non-toxic or low-toxic, environmentally friendly, does not contain materials such as asphalt, and has good environmental protection.

[0077] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing a fluid loss reducer for oil-based drilling fluid, It is characterized in that The following steps are involved: Polyvinyl pyrrolidone is added to a mixed solvent, nitrogen is introduced, and the mixture is stirred at room temperature; styrene, vinyl amide, unsaturated ester, and a cross-linking agent are then added and stirred evenly; an initiator is then added and heated for reaction; after the reaction is completed, the mixture is centrifuged, washed, and dried to obtain a fluid loss reducer for oil-based drilling fluid.

2. The method for preparing the fluid loss reducer for oil-based drilling fluid according to claim 1, It is characterized in that The following steps are involved: Polyvinyl pyrrolidone is added to a mixed solvent, nitrogen is introduced, and the mixture is stirred at room temperature; styrene, vinyl amide, unsaturated ester, modified inorganic material, and cross-linking agent are then added and stirred evenly; an initiator is then added and heated for reaction; after the reaction is completed, the mixture is centrifuged, washed, and dried to obtain a fluid loss reducer for oil-based drilling fluid.

3. The method for preparing the fluid loss reducer for oil-based drilling fluid according to claim 1, It is characterized in that The mixed solvent is a mixture of methanol and water; wherein the volume ratio of methanol to water is (5-8):(1-3).

4. The method for preparing the fluid loss reducer for oil-based drilling fluid according to claim 1, It is characterized in that The unsaturated ester is at least one of octadecyl methacrylate, isooctyl acrylate, n-butyl methacrylate, and ethyl 2-methacrylate.

5. The method for preparing the fluid loss reducer for oil-based drilling fluid according to claim 1, It is characterized in that The vinyl amide is N-vinyl caprolactam.

6. The method for preparing the fluid loss reducer for oil-based drilling fluid according to claim 1, It is characterized in that The crosslinking agent is pentaerythritol tetraacrylate.

7. The method for preparing the fluid loss reducer for oil-based drilling fluid according to claim 2, It is characterized in that The preparation method of the modified inorganic material comprises the following steps: The inorganic material and the silane coupling agent are added to the ethanol aqueous solution, mixed evenly, and heated to react. After the reaction is completed, the precipitate is centrifuged, washed, and dried to obtain a modified inorganic material.

8. The method for preparing the fluid loss reducer for oil-based drilling fluid according to claim 7, It is characterized in that The inorganic material is at least one of carbon microspheres and attapulgite.

9. The method for preparing the fluid loss reducer for oil-based drilling fluid according to claim 7, It is characterized in that The silane coupling agent is at least one of γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyltri(β-methoxyethoxy)silane and vinyltriethoxysilane.

10. A fluid loss reducer for oil-based drilling fluid, It is characterized in that Prepared by the preparation method according to any one of claims 1 to 9.