Preparation method of magnetically deformable high-solid-content hydrogel
By using polyvinyl alcohol and other materials to trigger polymerization reactions in magnetic responsive hydrogels, a high-solid content magnetic hydrogel with dual network structure is solved, and the brittleness and insufficient loading of existing magnetic responsive hydrogels are solved. Problem, high stability and excellent magnetic response deformation capability are achieved.
Patent Information
- Application Number
- CN202411051647.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The existing magnetic responsive hydrogels have high brittleness, low toughness, high strength, low elongation of fracture, and limited solid loading, resulting in slow magnetic response speed and low shape conversion efficiency of magnetic hydrogels.
Polyvinyl alcohol, acrylamide, N,N'-methylenebisacrylamide and potassium persulfate are used to cross-link in deionized water, and solid iron tetraoxide powder is added to trigger the polymerization reaction through dynamic cross-linking and heat. Construct a high-solid content magnetic hydrogel with a dual network structure.
It has achieved a magnetic particle load of up to 64%, has good structural stability of the hydrogel, has excellent magnetic response deformation ability and regulation performance, and improves the overall mechanical performance.
Smart Images

Figure CN118930744A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material preparation, and relates to a method for preparing a hydrogel, in particular to a method for preparing a high-solid-content magnetically deformable hydrogel. Background Art
[0002] Hydrogel is a polymer with a three-dimensional network structure obtained by cross-linking a macromolecule with a hydrophilic group. It can swell in water without dissolving, has a soft texture and adjustable properties. It can not only be equipped with various functions, such as magnetic, optical, electrical, thermal, humidity, pH and other stimulus responses, but also load different materials and transfer drugs, etc. It is one of the best choices for the substrate of flexible actuators. At present, magnetic responsive hydrogels with tissue penetration, contactless remote spatiotemporal control, and rapid reversible response have attracted extensive research and application in micro-robotics, tissue engineering, drug or cell transport and release, bionic actuators, and environmental governance due to their unique properties. However, most of the existing magnetic responsive hydrogels generally have problems such as high brittleness and low toughness, high strength and low elongation at break, and limited solid loading, which makes the magnetic response speed of magnetic hydrogel flexible brakes slow and the shape conversion efficiency low. Therefore, the development of new sensitive low-strength and high-loading magnetic responsive hydrogels from the perspective of materials and structures has become a key issue in the development of flexible intelligent magnetic responsive actuators.
[0003] At present, there are two main ways to improve the mechanical properties of magnetic hydrogels. One is to establish the interaction between magnetic particles and hydrogel substrate by modifying the functional groups on the surface of magnetic particles; the other is to introduce another cross-linking system into the magnetic hydrogel to form a double-network magnetic hydrogel. Based on the Hoffmeister effect and the toughening method of double-network hydrogels, researchers have prepared a Fe3O4 / CS (chitosan)-PAAm double-network electromagnetically conductive responsive hydrogel with ultra-high toughness through ionic crosslinking, molecular entanglement, and hydrogen bond enhancement between nanoparticles and polymer networks. The magnetic particle content can reach 43wt% (43% is relative to the total weight of polymer and water, which is converted to 30.07% of the total mass). The modulus of the prepared hydrogel is 1.3MPa and the toughness exceeds 54KJ / m 2The deformation of the gel can be adjusted by applying an external magnetic field, so that the gel has the function of a soft magnetic response actuator (MEI L, CONG J, LI S, et al. Polyacrylamide-Chitosanbased magnetic hydrogels with high stiffness and ultra-toughness[J]. Composites Part A: Applied Science and Manufacturing, 2023, 168: 107478.). In addition, the researchers compounded Fe3O4 nanoparticles coated with 3-(trimethoxysilyl)propyl methacrylate with polyacrylamide hydrogel to produce a magnetically responsive hydrogel with a magnetic powder content of up to 60wt% (37.5% of the total mass, relative to the total weight of polymer and water) and uniform distribution, relatively high modulus and toughness, and rapid response to magnetic fields. The hydrogel can adhere to hard and soft surfaces rich in hydroxyl groups. By coating the surface with polydimethylsiloxane, it can not only prevent the leakage of magnetic particles and dehydration, but also show excellent performance underwater (HU X, NIAN G, LIANG X, et al. Adhesive Tough Magnetic Hydrogels with High Fe3O4 Content[J].).
[0004] Although magnetically responsive hydrogel flexible brakes have made significant progress, there are still some difficulties and challenges in improving performance. For example, the goals of achieving high solid content and good dispersion of solid particles in hydrogels are often contradictory, and the mechanical properties of hydrogels gradually deteriorate with increasing solid content. Summary of the invention
[0005] In view of the common problems of existing magnetic hydrogels, such as high brittleness and low toughness, high strength and low elongation at break, and limited solid loading, the present invention provides a method for preparing magnetically deformable high-solid content hydrogels. The method is simple and easy to implement, and uses magnetic particles to give the gel magnetic responsiveness. Hydrogels of any shape can be constructed according to different molds, and the prepared double-network hydrogel has good mechanical properties and stability, and has a certain magnetic responsive deformation ability.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] A method for preparing a magnetically deformable high-solid content hydrogel comprises the following steps:
[0008] Step 1: adding polyvinyl alcohol to deionized water, heating and dissolving, to obtain a polyvinyl alcohol aqueous solution with a mass concentration of 3 to 15%;
[0009] Step 2: adding acrylamide, N,N'-methylenebisacrylamide and potassium persulfate in sequence to the polyvinyl alcohol aqueous solution obtained in step 1, and stirring to obtain a uniform solution, wherein: the amount of acrylamide added is 40-100% of the molar amount of the polyvinyl alcohol repeating unit, the amount of N,N'-methylenebisacrylamide added is 0.4-1% of the molar amount of acrylamide, and the amount of potassium persulfate added is 1-2% of the molar amount of acrylamide;
[0010] Step 3: Adding boric acid aqueous solution dropwise to the uniformly mixed solution obtained in step 2 while stirring to obtain a uniform dynamically cross-linked hydrogel, wherein: the concentration of the boric acid aqueous solution is 0.01-0.02 g / mL, the amount added is 0.4-2% of the molar amount of the polyvinyl alcohol repeating unit, and the stirring speed is 150-250 rpm;
[0011] Step 4: adding a small amount of ferroferric oxide solid powder to the dynamically cross-linked hydrogel obtained in step 3 in batches, stirring evenly and placing in a vacuum environment to remove bubbles, to obtain a dynamic reversible network hydrogel loaded with high-content magnetic particles, wherein: the speed of mechanical stirring is 100-200rpm, the particle size of ferroferric oxide is 50-500nm, and the amount of ferroferric oxide added is 10-64wt% of the dynamically cross-linked hydrogel obtained in step 3;
[0012] Step 5: The dynamic reversible network hydrogel obtained in step 4 is transferred to a polytetrafluoroethylene mold, and placed in an oven at 50 to 70° C. for thermal polymerization for 2 to 6 hours to obtain a magnetically deformable high-solid content hydrogel with good mechanical properties and stability.
[0013] Compared with the prior art, the present invention has the following advantages:
[0014] 1. The hydrogel constructed by the present invention has a magnetic particle loading capacity of up to 64%, and the structural stability of the hydrogel is good.
[0015] 2. The hydrogel constructed by the present invention has certain strength and toughness, and at the same time has excellent magnetic response deformation ability.
[0016] 3. The hydrogel constructed by the present invention has a wide adjustable range of performance. By rationally designing the ratio between the double networks and the content of each substance, the overall mechanical properties of the gel can be adjusted.
[0017] 4. The preparation method of the present invention is simple and easy to scale up for preparation. The operation process has strong stability and has practical application prospects and sustainability.
[0018] 5. The present invention is expected to develop hydrogel materials with high practical value in many fields, including but not limited to high solid content gel propellants, high solid content conductive hydrogels, high solid content magnetron gels, etc., showing important application potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 These are optical images of magnetic hydrogels with solid contents of approximately 20%, 55%, and 64%, respectively.
[0020] Figure 2 This is an infrared image of the magnetic hydrogel.
[0021] Figure 3 This is the SEM image of the hydrogel with a solid content of 64%.
[0022] Figure 4 It is the rotational rheometer oscillation amplitude scanning curve of the hydrogel precursor mixture with a solid content of 64%.
[0023] Figure 5 It is the rotational rheometer oscillation amplitude scanning curve of hydrogel with solid content of 64%.
[0024] Figure 6 This is the thermogravimetric curve of the double network hydrogel with a solid content of about 55%.
[0025] Figure 7 This is the thermogravimetric curve of the double network hydrogel with a solid content of about 64%. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is further described below in conjunction with the accompanying drawings, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.
[0027] The present invention provides a method for preparing a magnetically deformable high-solid content hydrogel, wherein polyvinyl alcohol is used as a raw material, first heated and dissolved in deionized water, then acrylamide, N,N'-methylenebisacrylamide and initiator potassium persulfate are added to the polyvinyl alcohol aqueous solution, and after all are dissolved, a boric acid aqueous solution is added dropwise while mechanically stirring, and then solid particles of ferrosoferric oxide are added, and stirred evenly to obtain a dynamic reversible network hydrogel loaded with a high content of solid particles, which is then transferred to a polytetrafluoroethylene mold and placed in a 60°C environment for thermal initiation, thereby constructing a double network hydrogel with excellent mechanical properties and a high content of magnetic particles. The specific steps are as follows:
[0028] Step 1: adding polyvinyl alcohol to deionized water, heating and dissolving, to obtain a polyvinyl alcohol aqueous solution with a mass concentration of 3 to 15%;
[0029] Step 2: adding acrylamide, N,N'-methylenebisacrylamide and potassium persulfate in sequence to the polyvinyl alcohol aqueous solution obtained in step 1, and stirring to obtain a uniform solution, wherein: the amount of acrylamide added is 40-100% of the molar amount of the polyvinyl alcohol repeating unit, the amount of N,N'-methylenebisacrylamide added is 0.4-1% of the molar amount of acrylamide, and the amount of potassium persulfate added is 1-2% of the molar amount of acrylamide;
[0030] Step 3: Adding boric acid aqueous solution dropwise to the uniformly mixed solution obtained in step 2 while stirring, to obtain a dynamically cross-linked hydrogel with a stable state and certain fluidity, wherein: the concentration of the boric acid aqueous solution is 0.01-0.02 g / mL, the amount added is 0.4-2% of the molar amount of the polyvinyl alcohol repeating unit, and the stirring speed is 150-250 rpm;
[0031] Step 4: adding a small amount of ferroferric oxide solid powder to the dynamically cross-linked hydrogel obtained in step 3 in batches, stirring evenly and placing in a vacuum environment to remove bubbles, to obtain a dynamic reversible network hydrogel loaded with high-content magnetic particles, wherein: the speed of mechanical stirring is 100-200rpm, the particle size of ferroferric oxide is 50-500nm, and the amount of ferroferric oxide added is 10-64wt% of the dynamically cross-linked hydrogel obtained in step 3;
[0032] Step 5: The dynamic reversible network hydrogel obtained in step 4 is transferred to a polytetrafluoroethylene mold, and placed in an oven at 50 to 70° C. for thermal polymerization for 2 to 6 hours to obtain a magnetically deformable high-solid content hydrogel with good mechanical properties and stability.
[0033] Embodiment 1:
[0034] At room temperature and pressure, 1g of polyvinyl alcohol is added to 12ml of deionized water, and the mixture is heated and stirred in an oil bath at 80°C to dissolve to obtain a polyvinyl alcohol aqueous solution; 2g of the polyvinyl alcohol aqueous solution is taken, and 0.3554g of acrylamide, 0.0039g of N,N'-methylenebisacrylamide, and 0.0135g of potassium persulfate are added thereto in sequence, and stirred to obtain a uniform solution; mechanical stirring is turned on, and 50μl of a 0.01g / ml boric acid aqueous solution is added, and the addition is divided into five times, and 10μl is taken and dripped in at a time using a pipette, and each time is 2.5 minutes apart, and the mixture is stirred until the state of the mixture is uniform; 4.21g of 500nm ferrosoferric oxide is added thereto in small amounts and multiple times, and mechanical stirring is stopped after the mixture is evenly mixed, and the mixture is placed in a vacuum environment to remove bubbles; the uniform mixture is then transferred to a polytetrafluoroethylene mold sprayed with a release agent, placed in a 60°C oven for thermal initiation of polymerization for 4 hours, and taken out from the mold to obtain a hydrogel with a specific shape, good mechanical properties, good stability, and a solid content of about 64%.
[0035] Embodiment 2:
[0036] At room temperature and pressure, 1g of polyvinyl alcohol is added to 10ml of deionized water, and the mixture is heated and stirred in an oil bath at 80°C to dissolve to obtain a polyvinyl alcohol aqueous solution; 2g of the polyvinyl alcohol aqueous solution is taken, and 0.3909g of acrylamide, 0.0042g of N,N'-methylenebisacrylamide, and 0.0149g of potassium persulfate are added thereto in sequence, and stirred to obtain a uniform solution; mechanical stirring is turned on, and 70μl of a 0.01g / ml boric acid aqueous solution is added, and the addition is divided into seven times, and 10μl is taken and dripped in at a time using a pipette, and each time is 2.5 minutes apart, and the mixture is stirred until the state of the mixture is uniform; 2.95g of 50nm ferrosoferric oxide is added thereto in small amounts and multiple times, and mechanical stirring is stopped after the mixture is evenly mixed, and the mixture is placed in a vacuum environment to remove bubbles; the uniform mixture is then transferred to a polytetrafluoroethylene mold sprayed with a release agent, placed in a 60°C oven for thermal initiation of polymerization for 4 hours, and taken out from the mold to obtain a hydrogel with a specific shape, good mechanical properties, good stability, and a solid content of about 55%.
[0037] Embodiment 3:
[0038] At room temperature and pressure, 1g of polyvinyl alcohol is added to 10ml of deionized water, and the mixture is heated and stirred in an oil bath at 80°C to dissolve to obtain a polyvinyl alcohol aqueous solution; 3g of the polyvinyl alcohol aqueous solution is taken, and 0.5864g of acrylamide, 0.0050g of N,N'-methylenebisacrylamide, and 0.0279g of potassium persulfate are added thereto in sequence, and stirred to obtain a uniform solution; mechanical stirring is turned on, and 90μl of a 0.01g / ml boric acid aqueous solution is added, and the addition is divided into nine times, and 10μl is dripped in at a time using a pipette, and each time is 2.5 minutes apart, and the mixture is stirred until the state of the mixture is uniform; 2.17g of 50nm ferrosoferric oxide is added thereto in small amounts and multiple times, and mechanical stirring is stopped after the mixture is evenly mixed, and the mixture is placed in a vacuum environment to remove bubbles; the uniform mixture is then transferred to a polytetrafluoroethylene mold sprayed with a release agent, and placed in a 60°C oven for thermal initiation of polymerization for 4 hours, and then taken out from the mold to obtain a hydrogel with a specific shape, good mechanical properties, good stability, and a solid content of about 37.5%.
[0039] Embodiment 4:
[0040] At room temperature and pressure, 1g of polyvinyl alcohol is added to 12ml of deionized water, and the mixture is heated and stirred in an oil bath at 80°C to dissolve to obtain a polyvinyl alcohol aqueous solution; 2.5g of the polyvinyl alcohol aqueous solution is taken, and 0.3554g of acrylamide, 0.0058g of N,N'-methylenebisacrylamide, and 0.0135g of potassium persulfate are added thereto in sequence, and stirred to obtain a uniform solution; mechanical stirring is turned on, and 100μl of a 0.01g / ml boric acid aqueous solution is added, and the addition is divided into 10 times, and 10μl is taken and dripped in at a time using a pipette, and each time is 2.5 minutes apart, and the mixture is stirred until the state of the mixture is uniform; 0.7190g of 500nm ferrosoferric oxide is added thereto in small amounts and multiple times, and mechanical stirring is stopped after the mixture is evenly mixed, and the mixture is placed in a vacuum environment to remove bubbles; the uniform mixture is then transferred to a polytetrafluoroethylene mold sprayed with a release agent, placed in a 55°C oven for thermal initiation of polymerization for 4h, and taken out from the mold to obtain a hydrogel with a specific shape, good mechanical properties, good stability, and a solid content of about 20%.
[0041] Depend on Figure 1 It can be seen that the magnetic hydrogels with solid contents of 20%, 55% and 64% respectively have stable and complete structures.
[0042] Depend on Figure 2 Visible, 1667cm -1 At 3450cm -1 There is a broad absorption band at 1351cm, which is caused by the stretching vibration of the -OH group on the polyvinyl alcohol. The full width at half maximum (FWHM) of this peak clearly shows the extensive hydrogen bonding between adjacent hydroxyl groups. The hydroxyl peak is red-shifted, indicating that hydrogen bonding is generated between the double network hydrogel and the magnetic particles. -1 The peak at 584cm is the borate ester bond peak after adding boric acid. -1 The peak of Fe-O stretching vibration after adding Fe3O4 is shown in Fig. 2. This proves the successful preparation of DN hydrogel and the introduction of magnetic particles into it.
[0043] Depend on Figure 3 It can be seen that the magnetic solid particles are densely loaded in the gel network, and no obvious hydrogel network structure can be seen. At the same time, no obvious stratification phenomenon is found, indicating that the solid particles are evenly dispersed.
[0044] Depend on Figure 4 It can be seen that the loss modulus is greater than the storage modulus, so the loss factor is greater than 1, and the mixed system exhibits partial fluid behavior, without a stable structure and a certain integrity. With the increase of shear stress, the modulus value increases, because the dynamic cross-linked network has a certain elasticity, and with the increase of shear stress, the climbing phenomenon occurs.
[0045] Depend on Figure 5It can be seen that after the chemical cross-linking network is formed, the storage modulus of the composite system is greater than the loss modulus, and is increased by about two orders of magnitude compared to the value before curing. The mixed system exhibits a solid-like behavior and has a certain stable structure and integrity.
[0046] Depend on Figure 6 , Figure 7 It can be seen that as the temperature gradually increases, the gel composite first undergoes desolventization and volatilization of small molecular components. At nearly 250°C, the polymer gradually begins to thermally degrade. At around 400°C, ferrosoferric oxide can be oxidized to iron oxide by oxygen in the air. At 800°C, the residue is mainly red iron oxide.
Claims
1. A method for preparing a magnetically deformable high-solid content hydrogel, characterized in that The method comprises the following steps: Step 1: adding polyvinyl alcohol to deionized water, heating and dissolving, to obtain a polyvinyl alcohol aqueous solution with a mass concentration of 3 to 15%; Step 2: adding acrylamide, N,N'-methylenebisacrylamide and potassium persulfate in sequence to the polyvinyl alcohol aqueous solution obtained in step 1, and stirring to obtain a uniform solution, wherein: the amount of acrylamide added is 40-100% of the molar amount of the polyvinyl alcohol repeating unit, the amount of N,N'-methylenebisacrylamide added is 0.4-1% of the molar amount of acrylamide, and the amount of potassium persulfate added is 1-2% of the molar amount of acrylamide; Step 3: Adding boric acid aqueous solution dropwise to the uniform mixed solution obtained in step 2 while stirring to obtain a uniform dynamic cross-linked hydrogel, wherein the amount of boric acid aqueous solution added is 0.4-2% of the molar amount of the polyvinyl alcohol repeating unit; Step 4: adding ferrosoferric oxide solid powder to the dynamic cross-linked hydrogel obtained in step 3, stirring evenly and placing in a vacuum environment to remove bubbles, thereby obtaining a dynamic reversible network hydrogel loaded with a high content of magnetic particles, wherein the amount of ferrosoferric oxide added is 10 to 64 wt % of the dynamic cross-linked hydrogel obtained in step 3; Step 5: The dynamic reversible network hydrogel obtained in step 4 is transferred to a polytetrafluoroethylene mold, and placed in an oven for thermally initiated polymerization for 2 to 6 hours to obtain a magnetically deformable high-solid content hydrogel with good mechanical properties and stability.
2. The method for preparing a magnetically deformable high-solid content hydrogel according to claim 1, characterized in that In the step 3, the concentration of the boric acid aqueous solution is 0.01 to 0.02 g / mL.
3. The method for preparing a magnetically deformable high-solid content hydrogel according to claim 1, characterized in that In the step 3, the stirring speed is 150-250 rpm.
4. The method for preparing a magnetically deformable high-solid content hydrogel according to claim 1, characterized in that In the step 4, the rotation speed of the mechanical stirring is 100-200 rpm.
5. The method for preparing a magnetically deformable high-solid content hydrogel according to claim 1, characterized in that In the step 4, the particle size of ferrosoferric oxide is 50 to 500 nm.
6. The method for preparing a magnetically deformable high-solid content hydrogel according to claim 1, characterized in that In the step 5, the oven temperature is 50-70°C.
Citation Information
Patent Citations
Method for preparing magnetic polymer microspheres by multiple emulsion method
CN104558353A
Quick-molding self-healing hydrogel and preparation method thereof
CN111393675A
Polyvinyl alcohol-based interpenetrating type gel
JP2019085521A